Water-based brilliant black fog burning and brightening treatment agent for synthetic leather and preparation method thereof

A technology of synthetic leather and treatment agent, applied in fiber treatment, flame retardant fibers, textiles and papermaking, etc., can solve the problems of poor gloss and color, unsatisfactory color development, poor storage stability, etc., and achieve clear color and luster. , The processing process is safe and reliable, and the compatibility is good.

Inactive Publication Date: 2017-02-01
JIANGSU BAOZE POLYMER MATERIAL
View PDF5 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] At present, the existing synthetic leather has poor hand feeling after being treated with water-based bright black mist ironing treatment agent, cracks when baked at high temperature, and the storage stability of the prepared spray dilution solution is poor, and the pigment is easy to settle
The synthetic leather applied with such a water-based bright black mist ironing and brightening treatment agent has poor luster and color, and the color development is not satisfactory.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Water-based brilliant black fog burning and brightening treatment agent for synthetic leather and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0029] The water-based bright black mist ironing treatment agent for synthetic leather contains 40 parts by mass of water-based resin, 2 parts by mass of water-based dispersant, 1 part by mass of defoamer, 10 parts by mass of silica matting powder, 1 part by mass of wetting agent, and 1 part by mass of Part of smooth feel agent, 1 part by mass of Deqian thickener, 40 parts by mass of water, 4 parts by mass of BCS.

[0030] The preparation method of the above-mentioned water-based bright black mist ironing treatment agent for synthetic leather is: 40 parts by mass of water-based resin in the formula, 2 parts by mass of water-based dispersant, 1 part by mass of defoamer, 10 parts by mass of silica matting powder, 1 part by mass of wetting agent, 1 part by mass of slippery feel agent, 1 part by mass of Deqian thickener, 40 parts by mass of water, and 4 parts by mass of BCS are uniformly stirred to obtain the synthetic leather with water-based brilliant black mist ironing treatmen...

Embodiment 2

[0033] The water-based treatment agent for synthetic leather includes 44 parts by mass of water-based resin, 1 part by mass of water-based dispersant, 0.5 parts by mass of defoamer, 8 parts by mass of silica matting powder, 0.5 parts by mass of wetting agent, and 0.5 parts by mass of Part of smooth feel agent, 0.5 parts by mass of Deqian thickener, 40 parts by mass of water, 5 parts by mass of BCS.

[0034] The preparation method of the above-mentioned water-based bright black mist ironing treatment agent for synthetic leather is: 44 parts by mass of water-based resin in the formula, 1 part by mass of water-based dispersant, 0.5 parts by mass of defoamer, 8 parts by mass of silica matting powder, 0.5 parts by mass of wetting agent, 0.5 parts by mass of slippery feel agent, 0.5 parts by mass of Deqian thickener, 40 parts by mass of water, and 5 parts by mass of BCS are uniformly stirred to obtain the described synthetic leather with water-based brilliant black mist ironing trea...

Embodiment 3

[0037] The water-based treatment agent for synthetic leather includes 44 parts by mass of water-based resin, 1 part by mass of water-based dispersant, 0.5 parts by mass of defoaming agent, 8.5 parts by mass of silica matting powder, and 0.5 parts by mass of smooth handle agent. 0.5 parts by mass of wetting agent, 0.5 parts by mass of Deqian thickener, 42.5 parts by mass of water, and 2 parts by mass of BCS.

[0038]The preparation method of the above-mentioned water-based bright black mist ironing and brightening treatment agent for synthetic leather is: 44 parts by mass of water-based resin in the formula, 1 part by mass of water-based dispersant, 0.5 parts by mass of defoaming agent, and 8.5 parts by mass of silica matting powder , 0.5 parts by mass of smooth hand agent, 0.5 parts by mass of wetting agent, 0.5 parts by mass of Deqian thickener, 42.5 parts by mass of water, and 2 parts by mass of BCS after uniform stirring to obtain the described synthetic leather water-based ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a water-based brilliant black fog burning and brightening treatment agent for synthetic leather and a preparation method thereof. The water-based brilliant black fog burning and brightening treatment agent for the synthetic leather is prepared from the following ingredients of water-based resin, a defoaming agent, silicon dioxide extinction powder, a wetting agent, a smooth feeling agent, a deuchem thickening agent, water and BCS. According to the water-based brilliant black fog burning and brightening treatment agent for the synthetic leather, all the ingredients are in intercoordination and combined action; the water-based brilliant black fog burning and brightening treatment agent has the advantages of being unique in hand feeling after treatment and free of crack when being roasted in a high temperature; meanwhile, prepared spray dilute solution has good storage stability, and pigment is not prone to deposite; the leather treated by the treatment agent is natural in gloss, clear in color, good in show color and excellent in comprehensive effect.

Description

technical field [0001] The invention relates to a water-based brilliant black mist ironing and brightening treatment agent for synthetic leather, in particular to a water-based brilliant black mist ironing and brightening treatment agent for synthetic leather used in the latter stage of the process. At the same time, the invention also discloses the synthetic leather water-based The invention discloses a preparation method of a brilliant black mist hot brightening treatment agent. Background technique [0002] At present, the existing synthetic leather has a poor hand feeling after being treated with a water-based bright black mist ironing treatment agent, and cracks when baked at high temperature. At the same time, the storage stability of the prepared spray dilution solution is poor, and the pigment is easy to settle. The synthetic leather that uses such water-based bright black mist ironing and brightening treatment agent has poor luster and color, and the color developme...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): D06M15/564D06M11/79
CPCD06M11/79D06M15/564D06M2200/30D06M2200/50
Inventor 陈勇刚
Owner JIANGSU BAOZE POLYMER MATERIAL
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products