A method for preparing purple sand craft ornaments from dust collected by filter bags of urban road sweepers
A technology for cleaning cars and dust, applied to clay products, other household utensils, household utensils, etc., can solve problems such as difficult handling, dust, and difficult molding, and achieve low cost, simple process, and fine texture.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] (1) Dust collection and pretreatment
[0024] Pour the dust collected by the filter bag of the urban road sweeper into the washing tank, add water 3 times the weight of the dust, stir in the washing tank for 8 minutes for washing, remove the floating objects on the water surface, filter and dry;
[0025] (2) Mature the purple sand raw material ore
[0026] The purple sand shale is selected as the raw material ore. The silicon dioxide content in the purple sand shale is 40wt%, the alumina content is 10wt%, the iron dioxide content is 40wt%, the titanium dioxide content is 0.2wt%, and the calcium oxide content is 1.5wt%. Under room temperature, the purple sand raw material ore is weathered to a water content of 10wt% in the purple sand raw material ore, and the weathered purple sand raw material ore is soaked with clear water, placed for 24 hours, and dried at 80°C to ripen it. The raw material ore is matured repeatedly 5 times; the raw purple sand ore is red purple sand...
Embodiment 2
[0036] (1) Dust collection and pretreatment
[0037] Pour the dust collected by the filter bag of the urban road sweeper into the washing tank, add water 5 times the weight of the dust, stir in the washing tank for 12 minutes for washing, remove the floating objects on the water surface, filter and dry;
[0038] (2) Mature the purple sand raw material ore
[0039] The purple sand shale is selected as the raw material ore. The silicon dioxide content in the purple sand shale is 35wt%, the alumina content is 12wt%, the iron dioxide content is 35wt%, the titanium dioxide content is 0.3wt%, and the calcium oxide content is 1.2wt%. , airing at room temperature to weatherize the purple sand raw material ore until the water content in the purple sand raw material ore is 10wt%, soak the weathered purple sand raw material ore with clear water, place it for 36 hours, and dry it at 100 ° C to mature it, and the weathered purple sand raw material ore The raw material ore is ripened repea...
Embodiment 3
[0049] (1) Dust collection and pretreatment
[0050] Pour the dust collected by the filter bag of the urban road sweeper into the washing tank, add water 4 times the weight of the dust, stir in the washing tank for 10 minutes for washing, remove the floating objects on the water surface, filter and dry;
[0051] (2) Mature the purple sand raw material ore
[0052] The purple sand shale is selected as the raw material ore. The silicon dioxide content in the purple sand shale is 30wt%, the alumina content is 15wt%, the iron dioxide content is 30wt%, the titanium dioxide content is 0.5wt%, and the calcium oxide content is 0.5wt%. Under room temperature, the purple sand raw material ore is weathered to a water content of 10wt% in the purple sand raw material ore, soaked with clear water after the weathered purple sand raw material ore, placed for 30h, and dried at 90°C to ripen it, and the weathered purple sand raw material ore is matured. The raw material ore is ripened repeated...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com