Rolling production method for improving toughness of steel on line

A production method and toughness technology, applied in the direction of metal rolling, metal rolling, manufacturing tools, etc., can solve the problems of undiscovered, undiscovered toughness, and improve the toughness of steel, so as to reduce heating energy consumption, protect the environment, and save production. cost effect

Active Publication Date: 2021-08-13
DAYE SPECIAL STEEL CO LTD
View PDF11 Cites 3 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] According to the literature search, in the prior art, for improving the toughness of steel, most iron and steel enterprises only improve the impact toughness of steel through the heat treatment process of quenched and tempered steel. At present, no research on hot-rolled steel has been found to improve the toughness of steel. There is also no relevant technical report on improving the toughness of steel by studying the rapid cooling of steel after rolling.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Rolling production method for improving toughness of steel on line
  • Rolling production method for improving toughness of steel on line

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0052] The rolling production method for improving the toughness of steel products on-line provided in this embodiment uses 40MnV non-adjusted steel continuous casting slab as raw material, and rolling production obtains a finished product 40MnV steel with a specification of 50mm. The rolling production method includes the following steps:

[0053] Step 1: Cut the 300×400×9000mm continuous casting slab and put it into the heating furnace by cold delivery or red delivery for reheating.

[0054] Step 2: Steel billet heating: adopt four-stage heating method to heat the steel billet, wherein the temperature of the second stage of heating meets the process requirements (ie 1100-1150°C); the temperature of the soaking section is 1160°C; the total heating in the heating process The time is 5h, and the soaking time in the soaking section is 70min.

[0055] Step 3: billet descaling: the heated billet is descaled with high-pressure water to remove scale; the pressure of the high-pressur...

Embodiment 2

[0065] The rolling production method for on-line improvement of steel toughness provided by this embodiment uses 40MnV non-adjusted steel continuous casting slab as raw material, and rolling production obtains a finished 40MnV steel bar with a specification of 85mm, including the following steps:

[0066] Step 1: Cut the 300×400×9000mm continuous casting slab and put it into the heating furnace by cold delivery or red delivery for reheating.

[0067] Step 2: Steel billet heating: adopt four-stage heating method to heat the steel billet, among which, the temperature of the preheating section is 590°C; the temperature of the heating stage is 1020°C; The temperature is 1150°C, which meets the process requirements; the total heating time in the heating process is 4.0h, and the soaking time in the soaking section is 78min.

[0068] Step 3: billet descaling: the heated billet is descaled by high-pressure water to remove scale, and the pressure of the high-pressure water is 50 MPa. ...

Embodiment 3

[0076] This embodiment provides a rolling production method for improving steel toughness on-line. Using 40MnV non-adjusted steel continuous casting slab as raw material, rolling production obtains a finished 40MnV steel bar with a specification of 75mm, including the following steps:

[0077] Step 1: Cut the 300×400×9000mm continuous casting slab and put it into the heating furnace by cold delivery or red delivery for reheating.

[0078] Step 2: Steel billet heating: adopt four-stage heating method to heat the steel billet, among which, the temperature of the preheating section is 580°C; the temperature of the heating section is 1020°C; The temperature is 1150°C, which meets the process requirements; the total heating time in the heating process is 5 hours, and the soaking time in the soaking section is 65 minutes.

[0079] Step 3: billet descaling: the heated billet is descaled by high-pressure water to remove scale, and the pressure of the high-pressure water is 50 MPa.

[0...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
crystal sizeaaaaaaaaaa
crystal sizeaaaaaaaaaa
Login to view more

Abstract

The invention discloses a rolling production method for improving the toughness of steel on line. A continuous casting billet is taken as a raw material. The rolling production method sequentially comprises the following working procedures of billet heating, descaling, rough rolling, continuous rolling, through-water cooling, finish rolling through a bar reducing and sizing mill and cooling through a cooling bed, and finally a finished product bar is obtained; wherein a rolled material subjected to continuous rolling is subjected to through-water cooling to 650-850 DEG C, after through-water cooling, the rolled material is subjected to self-tempering to obtain the finish rolling temperature of the bar reducing and sizing mill, the finish rolling temperature is 500-700 DEG C, and the temperature of the bar on the cooling bed is 480-650 DEG C. According to the method, KOCKS rolling is adopted for finish rolling of the bar reducing and sizing mill, proeutectoid ferrite in a non-required form is eliminated by controlling the finish rolling temperature and the cooling temperature after rolling, the toughness of the steel is improved, and the grain size, hardness and mechanical performance of the non-quenched and tempered steel can be controlled by adopting the rapid cooling technology after rolling.

Description

technical field [0001] The invention belongs to the field of special steel production and processing in the metallurgical industry, and relates to a rolling process, in particular to a method for improving the toughness of steel. Background technique [0002] In recent years, with the rapid development of my country's economy, my country's automobile manufacturing industry and machinery manufacturing industry have developed rapidly. In this context, the amount and variety of non-quenched and tempered steel are also increasing. also gradually increased. Non-quenched and tempered steel has better mechanical properties, more uniform hardness from the center to the edge, longer fatigue life, and greatly reduces manufacturing costs. It is widely used in the production of high-strength rods and shafts. However, due to the high final rolling temperature (generally 800-850°C) of non-quenched and tempered steel, the austenite grain size tends to be coarse, and it is easy to form pro-...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B21B1/18B21B45/00B21B45/02B21B45/08
CPCB21B1/18B21B45/004B21B45/0224B21B45/08
Inventor 曾庆博时涛李小龙黄国飘
Owner DAYE SPECIAL STEEL CO LTD
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products