[0010] Embodiment 1, a kind of drying method of piano plate, described steps are:
[0011] a. Put the selected plate into the drying kiln and heat it up. When the temperature rises from room temperature to 55°C dry bulb temperature and 47°C wet bulb temperature, preheat the plate;
[0012] b. Raise the plate to the predetermined processing temperature at a rate of 20°C / h dry bulb temperature and 16°C / h wet bulb temperature, keep the predetermined time for 4 hours and then start to cool down;
[0013] c. When the dry bulb temperature drops to 65°C and the wet bulb temperature is 57°C, maintain the medium condition, carry out humidity adjustment and balance treatment, and cool down and leave the kiln when the moisture content of the board is adjusted to 7% to 9%.
Embodiment 2
[0014] Embodiment 2, a kind of drying method of piano plate, described steps are:
[0015] a. Put the selected plate into the drying kiln and heat it up. When the temperature rises from room temperature to 58°C dry bulb temperature and 49°C wet bulb temperature, preheat the plate;
[0016] b. Raise the plate to the predetermined processing temperature at a rate of 20°C / h dry bulb temperature and 16°C / h wet bulb temperature, keep the predetermined time for 5 hours and then start to cool down;
[0017] c. When the dry bulb temperature drops to 68°C and the wet bulb temperature is 60°C, maintain the medium condition, carry out humidity adjustment and balance treatment, and cool down and leave the kiln when the moisture content of the board is adjusted to 7%.
Embodiment 3
[0018] Embodiment 3, a kind of drying method of piano plate, described steps are:
[0019] a. Put the selected plate into the drying kiln and heat it up. When the temperature rises from room temperature to 60°C dry bulb and 50°C wet bulb, preheat the plate;
[0020] b. Raise the plate to the predetermined processing temperature at a rate of 20°C / h dry bulb temperature and 16°C / h wet bulb temperature, and start to cool down after keeping the predetermined time for 6 hours;
[0021] c. When the dry bulb temperature drops to 70°C and the wet bulb temperature is 62°C, maintain the medium condition, carry out humidity adjustment and balance treatment, and cool down and leave the kiln when the moisture content of the board is adjusted to 8%.