A technology that pollutes soil and heavy metals. It is applied in the field of environmental engineering. It can solve the problems of unfavorable As fixation, no treatment method, and easy leaching of Pb, and achieve the effects of enhancing soil fertility, low cost, and strong metal adsorption capacity.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] 1) Weigh 33% fly ash, 34% lime, and 33% peat. The peat is first calcined in a muffle furnace at a high temperature of 450°C for 4.5 hours, and then fully pulverized and mixed by a ball mill to obtain heavy metals in contaminated soil. Hardener;
[0037] 2) Weigh 100g of Pb and As contaminated soil, add 10g of the above curing agent, stir evenly, add tap water with 40% (weight ratio) of the mixture, stir thoroughly for 10min, mix evenly, seal with film, and let stand for 15 days ;
[0038] 3) After 15 days, the cured body was leached by solid waste respectively. Toxic leaching method - acetic acid buffer solution method (HJ / T300-2007) to obtain the leachate, and the soil was measured by "Determination of Soil pH" (Agricultural Industry Standard NY / T 1377-2007) pH value.
[0039] After testing, the leaching concentration of Pb dropped from 34.1 mg / L before curing to 3.7 mg / L after curing, which was lower than the detection value, and the leaching concentration of As dr...
Embodiment 2
[0041] 1) Weigh 40% of fly ash, 40% of lime, and 20% of peat. The peat is first calcined in a muffle furnace at 450°C for 4.5 hours, and then fully pulverized and mixed by a ball mill to obtain heavy metals from contaminated soil. Hardener;
[0042] 2) Weigh 100g of Pb and As contaminated soil, add 15g of the above curing agent, stir evenly, add tap water with 40% (weight ratio) of the mixture, fully stir for 10min, mix evenly, seal with a film, and let it stand for 15 days ;
[0043] 3) After 15 days, the cured body was leached by solid waste respectively. Toxic leaching method - acetic acid buffer solution method (HJ / T300-2007) to obtain the leachate, and the soil was measured by "Determination of Soil pH" (Agricultural Industry Standard NY / T 1377-2007) pH value.
[0044]After testing, the leaching concentration of Pb dropped from 34.8 mg / L before curing to 3.5 mg / L after curing, which was lower than the detection value, and the leaching concentration of As dropped from 21...
Embodiment 3
[0046] 1) Weigh 33% fly ash, 51% lime, and 16% peat. The peat is calcined in a muffle furnace at a high temperature of 450°C for 4.5 hours, and then fully pulverized and mixed by a ball mill to obtain heavy metals from contaminated soil. Hardener;
[0047] 2) Weigh 100g of Pb and As contaminated soil, add 10g of the above curing agent, stir evenly, add tap water with 40% (weight ratio) of the mixture, stir thoroughly for 10min, mix evenly, seal with film, and let stand for 15 days ;
[0048] 3) After 15 days, the cured body was leached by solid waste respectively. Toxic leaching method - acetic acid buffer solution method (HJ / T300-2007) to obtain the leachate, and the soil was measured by "Determination of Soil pH" (Agricultural Industry Standard NY / T 1377-2007) pH value.
[0049] After testing, the leaching concentration of Pb dropped from 34.6 mg / L before curing to 2.8 mg / L after curing, which was lower than the detection value, and the leaching concentration of As droppe...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com