A technology of composite plastic and remote control, applied in the field of remote control, can solve the problems of large molecular rigidity and steric hindrance, difficult to make large thin-walled remote control shell, etc., to improve surface smoothness and thermal stability, improve resistance Scratch performance, good weather resistance effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0018] A method for preparing an ABS composite plastic for an air conditioner remote control shell, comprising the following steps:
[0019] S1. Mix polyphosphoric acid, tetrahydrofuran-oxypropylene copolymer glycol, heat up and stir, add bisphenol F epoxy resin and continue stirring, add phthalic anhydride, trimethylolpropane trimethacrylate, heat up and stir, Cool and pulverize to obtain prefabricated material a;
[0020] S2. Mix ABS resin, polycarbonate resin, polystyrene, and preform a uniformly to obtain preform b;
[0021] S3. Add talcum powder, trichloroethyl phosphate, pine tar, and antioxidant B215 to the prefabricated material b, stir, and send it into a twin-screw extruder to extrude and granulate to obtain an ABS composite plastic for an air conditioner remote control shell.
Embodiment 2
[0023] A method for preparing an ABS composite plastic for an air conditioner remote control shell, comprising the following steps:
[0024] S1. Mix 15 parts of polyphosphoric acid and 30 parts of tetrahydrofuran-propylene oxide copolymerized glycol in parts by weight, raise the temperature to 85°C and stir for 2 hours, add 60 parts of bisphenol F epoxy resin and continue stirring for 12 minutes, add 1 part of phthaloxylene Acid anhydride, 0.8 parts of trimethylolpropane trimethacrylate, heated up to 145°C and stirred for 50 minutes, cooled and pulverized to obtain preform a;
[0025] S2. Mix 40 parts of ABS resin, 30 parts of polycarbonate resin, 15 parts of polystyrene, and 6 parts of preform a in parts by weight to obtain preform b;
[0026] S3. Add 18 parts of talcum powder, 1 part of trichloroethyl phosphate, 2 parts of pine tar, and 1 part of antioxidant B215 to 80 parts of prefabricated material b by weight and stir for 10 minutes at a stirring speed of 2000r / min. Extr...
Embodiment 3
[0028] A method for preparing an ABS composite plastic for an air conditioner remote control shell, comprising the following steps:
[0029] S1. Mix 35 parts of polyphosphoric acid and 10 parts of tetrahydrofuran-propylene oxide copolymerized glycol in parts by weight, raise the temperature to 95°C and stir for 1 hour, add 80 parts of bisphenol F epoxy resin and continue stirring for 4 minutes, and add 2 parts of phthalene Acid anhydride, 0.2 parts of trimethylolpropane trimethacrylate, heated to 165°C and stirred for 30 minutes, cooled and pulverized to obtain preform a;
[0030] S2. Mix 80 parts of ABS resin, 20 parts of polycarbonate resin, 25 parts of polystyrene, and 2 parts of preform a in parts by weight to obtain preform b;
[0031] S3. Add 10 parts of talcum powder, 2 parts of trichloroethyl phosphate, 1 part of pine tar, and 2 parts of antioxidant B215 to 100 parts of prefabricated material b by weight and stir for 5 minutes at a stirring speed of 2400r / min. Extrude...