Embodiment 1
[0024] 120g / m 2 The preparation method of double-layer structural paper with white surface and blue background, which is produced by two rotary screens and two sets of sizing system structural paper machines, and the sizing flow delivery system of one rotary screen paper machine is blue pulp, and the weight is 70g / m on the Internet. 2 , the other part of the sizing and flow delivery system of the rotary paper machine is white paper, and the weight is 50g / m on the Internet. 2 , and include the following steps:
[0025] (1) Ratio of pulp in the circular wire section of white tissue paper: 30% of softwood pulp from Kelly, 20% of hardwood pulp from Rizhao, and 50% of SWP fiber. The coniferous wood pulp and hardwood pulp are mixed and beaten by double disc mills, the beating degree is 55±1oSR, and the wet weight is 6.0-6.5g. SWP fibers are disintegrated using a hydropulper. The dosage of AKD sizing agent is 0.7%, the dosage of PAE wet strength agent is 1.0%, the dosage of cation...
Embodiment 2
[0029] 180g / m 2 The preparation method of double-layer structure paper with white surface and gray bottom, which adopts a Fourdrinier and one rotary wire structure, and is produced by two paper machines with sizing system. 2 , the sizing flow system part of the rotary screen is white paper, and the weight is 50g / m on the Internet. 2 , and include the following steps:
[0030] (1) Ratio of pulp in the circular wire section of white tissue paper: 30% of softwood pulp from Kelly, 20% of hardwood pulp from Rizhao, and 50% of SWP fiber. The coniferous wood pulp and hardwood pulp are mixed and beaten by double disc mills, the beating degree is 55±1oSR, and the wet weight is 6.0-6.5g. SWP fibers are disintegrated using a hydropulper. The dosage of AKD sizing agent is 0.7%, the dosage of PAE wet strength agent is 1.0%, the dosage of cationic starch in pulp is 1.2%, and the dosage of polyacrylamide retention aid is 100PPM.
[0031] (2) The pulp ratio of the fourdrinier part of the ...
Embodiment 3
[0034] The difference between this embodiment and Example 1 is that in the surface layer paper, by weight, softwood pulp and hardwood pulp are calculated as 20 parts by absolute dry weight, and the proportion of SWP fiber is calculated by total absolute dry weight. The total fiber weight is 80 parts.