Special paper with stable size and excellent restorability and preparation method thereof
A dimensionally stable and restorative technology, applied in the field of papermaking, can solve the problems that the deformed shape such as foaming and wrinkles cannot be improved, cannot be restored to a flat shape, the smoothness of the wallpaper surface, and the appearance is deteriorated, so as to improve the stability of cross-linking. The effect of improving recovery and relieving swelling and deformation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] The paper includes wood pulp fiber 60, mineral filler 3, wetting agent 3 and defoamer 2 in parts by mass, and is characterized in that it also includes aminosilane 5 and sugar alcohol 5.
[0016] The general formula of sugar alcohol is HOCH 2 [CH(OH)] 3 CH 2 Oh
[0017] Wood pulp fibers include coniferous pulp and hardwood pulp, and the mass ratio of coniferous pulp to hardwood pulp is 50:50.
[0018] The aminosilane is γ-aminopropyltrimethoxysilane.
[0019] The preparation method is as follows: take wood pulp fiber, mineral filler, wetting agent, defoamer, aminosilane, and sugar alcohol according to the above formula and add them to a pulper for pulping, and then refine the pulp. After papermaking, surfing, pressing, drying, Calendering, rolling, cutting and packaging are all you need.
Embodiment 2
[0021] The paper includes wood pulp fiber 70, mineral filler 4, wetting agent 4 and defoamer 4 in parts by mass, and is characterized in that it also includes aminosilane 8 and sugar alcohol 8.
[0022] The general formula of sugar alcohol is HOCH 2 [CH(OH)] 4 CH 2 Oh
[0023] Wood pulp fibers include coniferous pulp and hardwood pulp, and the mass ratio of coniferous pulp to hardwood pulp is 40:60.
[0024] The aminosilane is γ-aminopropyltriethoxysilane.
[0025] The preparation method is as follows: take wood pulp fiber, mineral filler, wetting agent, defoamer, aminosilane, and sugar alcohol according to the above formula and add them to a pulper for pulping, and then refine the pulp. After papermaking, surfing, pressing, drying, Calendering, rolling, cutting and packaging are all you need.
Embodiment 3
[0027] The paper includes wood pulp fiber 80, mineral filler 5, wetting agent 5 and defoamer 5 in parts by mass, and is characterized in that it also includes aminosilane 10 and sugar alcohol 10.
[0028] The general formula of sugar alcohol is HOCH 2 [CH(OH)] 5 CH 2 Oh
[0029] Wood pulp fibers include coniferous pulp and hardwood pulp, and the mass ratio of coniferous pulp to hardwood pulp is 60:40.
[0030] The aminosilane is N-β(aminoethyl)-γ-aminopropyltrimethoxysilane.
[0031] The preparation method is as follows: take wood pulp fiber, mineral filler, wetting agent, defoamer, aminosilane, and sugar alcohol according to the above formula and add them to a pulper for pulping, and then refine the pulp. After papermaking, surfing, pressing, drying, Calendering, rolling, cutting and packaging are all you need.