Process for coloring rubber material surface

A process method and surface coloring technology, applied in the field of industrial model manufacturing, can solve the problems of cracking, falling off, monotony, etc., and achieve the effect of high impact strength

Active Publication Date: 2009-07-29
BEIJING KINGCO TECH DEV
View PDF2 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The rubber material is characterized by flexibility, wear resistance, soft surface light, and good hand feeling; but in terms of craftsmanship, rubber coloring has always been very limited. The existing method is to directly add rubber coloring materials to the For pouring glue, get the corresponding color after pouring and drying
In this way, only a few monotonous basic colors are obtained, which cannot meet the strong demand of the market at all.
Therefore, the disadvantage of rubber materials is that there are few color varieties, especially the multiple colors that can not be flexibly and accurately selected on the surface of model parts according to the requirements of model design and the needs of users.
In the prior art, the rubber material is colored by simply spraying paints of various colors on the rubber surface. Since the rubber itself is an elastic material, during production and use, the rubber parts must often be stretched, compressed, bent, etc. by various external forces. Deformation, when the paint is directly sprayed on the rubber surface, its adhesion is difficult to meet the requirements
Because paint and rubber are not compatible with each other, and the elastic coefficient of general paint is smaller than that of rubber, when the rubber part is elastically deformed by external force, the paint attached to the rubber surface will also be deformed. When the elastic deformation of the paint exceeds its own elastic limit, it must be It will fall off, which makes it difficult to attach the paint coating on the rubber surface, and often cracks or even falls off, which directly affects the beauty and strength of the model surface

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0014] (1) Clean up the inside of half of the silicone mold on the appearance surface of the rubber product to be made;

[0015] (2) In a clean space at normal temperature and pressure, spray the prepared silver-white product surface paint on the inner surface of the mold on the outer surface of the product. The thickness of the paint film is 5 microns, and the excess paint around the mold is removed, leaving only Paint on the inner surface of the lower mold;

[0016] (3) After the above-mentioned paint that has been sprayed on the inner surface of the product appearance surface mold is left naturally for 5 minutes, start to pour the rubber for making the product in the mold, and the pouring pressure is 85 kPa;

[0017] (4) Make the poured rubber product and its mold stay in the vacuum machine for 50 seconds, then take it out and put it into the oven for baking, the baking temperature is controlled at 60°C, and the baking time is 2 hours;

[0018] (5) Put the above-mentioned ...

Embodiment 2

[0020] (1) Clean up the inside of half of the silicone mold on the appearance surface of the rubber product to be made;

[0021] (2) In a clean space at normal temperature and pressure, spray the prepared dark gray product surface paint on the inner surface of the mold on the product appearance surface. The thickness of the paint film is 25 microns, and remove the excess paint around the mold, leaving only The paint on the inner surface of the silicone mold on half of the outer surface of the product;

[0022] (3) After placing the above-mentioned paint sprayed on the inner surface of the product appearance surface mold for 7 minutes, start pouring the rubber for making the product in the mold, and the pouring pressure is 95 kPa;

[0023] (4) After making the poured rubber product and its mold stay in the vacuum machine for 70 seconds, take it out and put it into the oven for baking, the baking temperature is controlled at 75°C, and the baking time is 3.2 hours;

[0024] (5) ...

Embodiment 3

[0026] (1) Clean up the inside of half of the silicone mold on the appearance surface of the rubber product to be made;

[0027] (2) In a clean space at normal temperature and pressure, spray the prepared dark blue product surface paint on the inner surface of the mold on the product appearance surface. The thickness of the paint film is 40 microns, and remove the excess paint around the mold, leaving only The paint on the inner surface of the silicone mold on half of the outer surface of the product;

[0028] (3) After the above-mentioned paint that has been sprayed on the inner surface of the product appearance surface mold is left naturally for 10 minutes, start to pour the rubber for making the product in the mold, and the pouring pressure is 130 kPa;

[0029] (4) After making the poured rubber product and its mold stay in the vacuum machine for 90 seconds, take it out and put it into the oven for baking, the baking temperature is controlled at 85°C, and the baking time is...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
Login to View More

Abstract

The invention relates to a process method for coloring the surface of a rubber material, which comprises the following steps: cleaning the inside of the half-side silicone mold of the appearance surface of the product to be produced, and spraying the surface paint of the product on the mold of the appearance surface at normal temperature and pressure The inner surface, with a thickness of 5 to 40 microns, is naturally placed for 5 to 10 minutes, and the rubber is poured into the mold at a pressure of 85 to 130 kPa, so that the cast rubber product and its mold stay in the vacuum machine for 50 seconds to 90 Seconds later, take it out and bake in an oven at 60°C to 85°C for 2 to 4 hours, then place the product in a refrigerator at a temperature of 0°C to 10°C to cool down for 20 to 40 minutes, after curing, open the mold and take it out; The above process is used to color the rubber surface, which can accurately select the color according to the design requirements, and prevent the color attached to the surface of the rubber product from cracking, and has high impact resistance.

Description

technical field [0001] The invention relates to the field of industrial model manufacturing, in particular to a process method for coloring the surface of rubber materials. technical background [0002] With the advancement of science and technology and the development of industrial model manufacturing, there are more and more models with rubber layers on the surface of these materials, directly using rubber materials to make models or using other materials to make models. The rubber material is characterized by flexibility, wear resistance, soft surface light, and good hand feeling; but in terms of craftsmanship, rubber coloring has always been very limited. The existing method is to directly add rubber coloring materials to the For pouring glue, get the corresponding color after pouring and drying. In this way, only a few monotonous basic colors are obtained, which cannot meet the strong demand of the market at all. Therefore, the disadvantage of the rubber material is t...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): B29C39/10B29C39/44B29C39/38B29C39/22B29C35/00
Inventor 杜星武
Owner BEIJING KINGCO TECH DEV