Needle coke raw material evaluation method
A technology of needle coke raw material and evaluation method, which is applied in the field of needle coke raw material evaluation, can solve the problems of inability to judge whether petroleum-based raw materials are mixed with coal-based components, and the analysis process is time-consuming and labor-intensive.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] Material
[0022] The needle coke petroleum raw material sample to be tested is catalytic cracking oil slurry from refinery A.
[0023] The standard petroleum raw material is catalytic cracking oil slurry from Yangzhou Petrochemical Co., Ltd., and the filter paper is Φ12.5 quantitative filter paper (medium speed 202, Whatman).
[0024] This embodiment provides a needle coke raw material evaluation method, which includes the following steps:
[0025] a) Take the filter paper soaked and dried in toluene, place it in a weighing bottle, and dry it at 115-120°C to constant weight;
[0026] b) Add 10mL of the needle coke petroleum raw material to be tested and 40mL of naphtha into a 100mL reaction beaker, place the beaker in a water bath at 40°C, and stir for 2 minutes;
[0027] c) Suction-filtering the mixture obtained in step b) on the filter paper obtained in step a), and the precipitate remains on the filter paper;
[0028] d) Wash the reaction beaker (20mL x 3) with n...
Embodiment 2
[0033] Material
[0034] The needle coke petroleum raw material to be tested is FCC oil slurry from Refinery B.
[0035] Other materials are the same as in Example 1.
[0036] This embodiment provides a needle coke raw material evaluation method, which includes the following steps:
[0037] a) Take the filter paper soaked and dried in toluene, place it in a weighing bottle, and dry it at 115-120°C to constant weight;
[0038] b) Add 10mL of the needle coke raw material to be tested and 40mL of gasoline into a 100mL reaction beaker, place the beaker in a 60°C water bath, and stir for 5 minutes;
[0039] c) Suction-filtering the mixture obtained in step b) on the filter paper obtained in step a), and the precipitate remains on the filter paper;
[0040] d) Wash the reaction beaker (20mL x 3) with gasoline at 60°C, transfer the remaining precipitate to the filter paper, filter with suction, and wash the precipitate on the filter paper with 40mL gasoline;
[0041] e) Dry the f...