Since the temperature of the lead pool in the lead furnace is generally set at 460-500°C during casting and welding, and some batteries require it to be set at 530°C, the cork powder component of the release agent is easily carbonized at such a high temperature, which makes the release agent last longer. , casting and welding workers need to frequently add release agent, which is time-consuming and laborious, and the production efficiency is low

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0028] Measure 4500mL of tap water (equivalent to 4500g of water) and 204mL of sodium silicate (the density of sodium silicate is 2.33g / mL, equivalent to 476g of sodium silicate), put them in a heating pot with a stirrer, and mix the tap water and sodium silicate The mixture was heated to boiling at a stirring speed of 50 rpm, and then continued to stir and heat to boil for 25 minutes. Then, add the 100 order cork powder of 476g in heating pot, continue to stir heating and boil 25 minutes. Then, add 48g of diatomaceous earth in heating pot, continue to stir heating and boil for 45 minutes. Then, 4500 mL of tap water was added to the heating pot, the heating was stopped, and stirring was continued until the reaction mixture reached normal temperature. Finally, the reaction mixture was allowed to stand for 10 minutes, and the milky white suspension in the upper layer was taken after the layers were separated to obtain a mold release agent for casting and welding.

[0029] Cons...

Embodiment 2

[0031] Measure 4250mL tap water (equivalent to 4250g water) and 303mL sodium silicate (equivalent to 706g sodium silicate), place in a heating pot with a stirrer, heat the mixture of tap water and sodium silicate to boiling at a stirring speed of 50rpm, Continue to stir and heat to boil for 20 minutes. Then, add the 100 order cork powder of 706g in heating pot, continue to stir heating and boil 20 minutes. Then, add 88g of diatomaceous earth in the heating pot, continue stirring and heating and boiling for 30 minutes. Then, 4250 mL of tap water was added to the heating pot, the heating was stopped, and stirring was continued until the reaction mixture reached normal temperature. Finally, the reaction mixture was allowed to stand for 10 minutes, and the milky white suspension in the upper layer was taken after the layers were separated to obtain a mold release agent for casting and welding.

[0032] Considering that the moisture loss in the process of boiling and stirring is ...

Embodiment 3

[0034] Measure 4750mL tap water (equivalent to 4750g water) and 97.4mL sodium silicate (equivalent to 227g sodium silicate), place in a heating pot with a stirrer, heat the mixture of tap water and sodium silicate to boiling at a stirring speed of 50rpm , continue to stir and boil for 30 minutes. Then, add 100 order cork powders of 227g in the heating pot, continue to stir and heat and boil for 30 minutes. Then, add 46g diatomaceous earth in heating pot, continue to stir heating and boil for 60 minutes. Then, 4750 mL of tap water was added to the heating pot, the heating was stopped, and stirring was continued until the reaction mixture reached normal temperature. Finally, the reaction mixture was allowed to stand for 10 minutes, and the milky white suspension in the upper layer was taken after the layers were separated to obtain a mold release agent for casting and welding.

[0035] Considering that the moisture loss in the process of boiling and stirring is about 10%, the ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Granularityaaaaaaaaaa
Densityaaaaaaaaaa
Login to View More

Abstract

The invention relates to a cast-weld release agent. The agent comprises water, sodium silicate, cork powder and diatomaceous earth, wherein the mass of water accounts for 85% of the total mass of thecast-weld release agent, and the mass ratio of the sodium silicate to the cork powder to the diatomaceous earth is (5-10): (5-10):1. The particle size of the cork powder is preferably 100 meshes or above. The invention further provides a preparation method of the cast-weld release agent. The method comprises the following steps that half of the formula amount of the water and the formula amount ofthe sodium silicate are heated and boiled under stirring, the formula amount of cork powder is added, the mixture is continuously heated and boiled under stirring, then the formula amount of diatomite is added, the mixture is continuously heated and boiled under stirring, then the other half of the formula amount of water is added, stirring is continuously conducted until the mixture reaches theambient temperature, the reactant is left to stand, and an upper-layer suspension is taken after layering to obtain the cast-weld release agent. According to the cast-weld release agent, the strippingefficiency can be improved, by adding the diatomaceous earth in a small amount, the cork powder can be adsorbed, the carbonization rate of the cork powder can be delayed, and the continuous service time of the release agent can be prolonged.

Description

technical field [0001] The invention relates to the technical field of lead-acid storage batteries, in particular to a novel mold release agent for casting and welding and a preparation method thereof. The novel mold release agent for casting and welding is especially applicable to the mold release of busbars of lead-acid storage batteries. Background technique [0002] In the manufacture of lead-acid batteries, it is necessary to form a busbar by performing lug casting and welding to connect the lead-acid battery plates in parallel. The quality of the busbar casting and welding directly affects the quality of the lead-acid battery. During casting and welding, high-temperature lead liquid at 460-500°C flows into the mold cavity of the busbar mold. The lead liquid melts the surface of the pole plate lug by virtue of its high temperature, and then passes water in the mold to cool the mold quickly to form the busbar. , and finally the busbar is detached from the mold cavity by ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): B22C3/00B22D19/04B22D25/04
CPCB22C3/00B22D19/04B22D25/04
Inventor杨金辉刘春张建华
OwnerJIANGSU LEOCH BATTERY