Color aluminum plate water-based paint of water-based polyester acrylate resin and preparation method thereof
A polyester acrylate and board water-based technology, applied in polyester coatings, coatings, etc., can solve the problems of single function and insufficient practicability, and achieve the effects of beautifying the environment, avoiding drug residues, and protecting human health
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] In the embodiment of the present invention, a water-based paint for color aluminum plate of water-based polyester acrylate resin and its preparation method, its raw materials include the following components by weight: 40 parts of water-based polyester acrylate resin, 35 parts of deionized water, amino 2 parts of resin, 10 parts of titanium dioxide, 3 parts of film forming agent, 4 parts of defoamer, 6 parts of dispersant, 3 parts of thickener, 3 parts of antifreeze, 1 part of PH regulator, 7 parts of contact killer, solubilizer 3 parts, 3 parts synergist.
[0029] The specific steps are as follows:
[0030] Step 1: Add water, water-based polyester acrylate resin, and titanium dioxide to the stirring machine with heating function in sequence;
[0031] Step 2: Start the stirring machine and stir for 20-40 minutes at a temperature of 40-50°C. The rotation speed of the stirring blade is 200-400r / min. During the stirring process, add a dispersant to the stirring machine. A...
Embodiment 2
[0038] In the embodiment of the present invention, a water-based paint for color aluminum plate of water-based polyester acrylate resin and its preparation method, its raw materials include the following components in parts by weight: 35 parts of water-based polyester acrylate resin, 30 parts of deionized water , 1 part of amino resin, 11 parts of titanium dioxide, 2 parts of film forming agent, 3 parts of defoamer, 5 parts of dispersant, 2 parts of thickener, 2 parts of antifreeze, 2 parts of PH regulator, contact killer, solubilizer 2 parts, 2 parts synergist.
[0039] The specific steps are as follows:
[0040] Step 1: Add water, water-based polyester acrylate resin, and titanium dioxide to the stirring machine with heating function in sequence;
[0041] Step 2: Start the stirring machine and stir for 20-40 minutes at a temperature of 40-50°C. The rotation speed of the stirring blade is 200-400r / min. During the stirring process, add a dispersant to the stirring machine. Af...
Embodiment 3
[0048] In the embodiment of the present invention, a water-based paint for color aluminum plate of water-based polyester acrylate resin and its preparation method, its raw materials include the following components by weight: 45 parts of water-based polyester acrylate resin, 40 parts of deionized water , 2 parts of amino resin, 12 parts of titanium dioxide, 4 parts of film forming agent, 4 parts of defoamer, 8 parts of dispersant, 4 parts of thickener, 4 parts of antifreeze, 3 parts of pH regulator, 9 parts of contact killer, 3 parts of solubilizer, 3 parts of synergist.
[0049] The specific steps are as follows:
[0050]Step 1: Add water, water-based polyester acrylate resin, and titanium dioxide to the stirring machine with heating function in sequence;
[0051] Step 2: Start the stirring machine and stir for 20-40 minutes at a temperature of 40-50°C. The rotation speed of the stirring blade is 200-400r / min. During the stirring process, add a dispersant to the stirring mac...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology