Efficient retarding and water reducing agent for cement concrete and preparation method of efficient retarding and water reducing agent
A retarding water reducer and cement concrete technology, applied in the field of water reducer, can solve the problems of accelerated concrete loss, reduced concrete strength, prolonged setting time, etc., to improve workability and fluidity, improve concrete structure, increase The effect of retarding effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] A high-efficiency retarding water reducer for cement concrete, comprising the following raw materials in parts by mass: 80 parts of polyethylene glycol methyl ether methacrylate, 20 parts of methacrylic acid, 40 parts of 2-hydroxyphosphonoacetic acid, 10 parts of acid anhydride, 10 parts of phosphoric acid slow release agent, 2 parts of initiator, 3 parts of chain transfer agent, 150 parts of deionized water;
[0037] The preparation method of the water reducing agent comprises the following steps:
[0038] Step 1: Use 30ml / min of high-purity nitrogen to evacuate the air in the reactor, take mass parts of maleic anhydride and 2-hydroxyphosphonoacetic acid into the reactor, and use 30ml / min of high-purity nitrogen to ventilate again into the reaction kettle for 20 minutes; then the temperature was heated to 60°C, while stirring at a speed of 300r / min, the reaction was carried out for 1 hour, the stirring was stopped, and then naturally cooled to room temperature to obtai...
Embodiment 2
[0042] A high-efficiency retarding water reducer for cement concrete, comprising the following raw materials in parts by mass: 100 parts of polyethylene glycol methyl ether methacrylate, 30 parts of methacrylic acid, 70 parts of 2-hydroxyphosphonoacetic acid, Malay 20 parts of acid anhydride, 30 parts of phosphoric acid slow release agent, 3 parts of initiator, 5 parts of chain transfer agent, 300 parts of deionized water;
[0043]The preparation method of the water reducing agent comprises the following steps:
[0044] Step 1: Use 50ml / min of high-purity nitrogen to evacuate the air in the reactor, take mass parts of maleic anhydride and 2-hydroxyphosphonoacetic acid into the reactor, and use 50ml / min of high-purity nitrogen to ventilate again into the reaction kettle for 30 minutes; then the temperature was heated to 80°C, while stirring at a speed of 500r / min, the reaction was carried out for 2 hours, the stirring was stopped, and then naturally cooled to room temperature t...
Embodiment 3
[0048] A high-efficiency retarding water reducer for cement concrete, comprising the following raw materials in parts by mass: 90 parts of polyethylene glycol methyl ether methacrylate, 25 parts of methacrylic acid, 55 parts of 2-hydroxyphosphonoacetic acid, 15 parts of acid anhydride, 20 parts of phosphoric acid slow release agent, 2 parts of initiator, 4 parts of chain transfer agent, 200 parts of deionized water;
[0049] The preparation method of the water reducing agent comprises the following steps:
[0050] Step 1: Use 40ml / min of high-purity nitrogen to evacuate the air in the reactor, take mass parts of maleic anhydride and 2-hydroxyphosphonoacetic acid into the reactor, and use 40ml / min of high-purity nitrogen to ventilate again into the reaction kettle for 25 minutes; then the temperature was heated to 70°C while stirring at a speed of 400r / min for 1.5 hours, the stirring was stopped, and then naturally cooled to room temperature to obtain a phosphate ester modified...