Wall material for geomagnetic functional house, preparation method and functional house
A technology for wall materials and functional rooms, applied in the field of functional rooms, to achieve the effects of improving stability, improving magnetism, and good magnetic therapy
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2022-05-24
Smart Images

Figure 1 
Figure 2
Abstract
Description
technical field
[0001] The invention relates to the technical field of functional building materials, in particular to a wall material and a preparation method for a geomagnetic functional room, and a functional room. Background technique
[0002] Walls are an important part of buildings. Traditional wall materials include natural stone, functional artificial slate, and functional wall coatings. Different wall materials have a key impact on the exterior decoration effect and internal environment of the building. With the continuous improvement of wall materials, more and more different types of new wall materials have gradually emerged, which often have excellent mechanical and chemical properties, such as thermal insulation, waterproof and moisturizing, sound insulation and noise reduction and other properties.
[0003] At present, the wall materials are developing towards green environmental protection and multi-functionality, and the research on functional wall materials ...
Examples
Embodiment 1
[0032] A wall material for a geomagnetic function room, according to the ratio of parts by mass, including 8 parts of black tourmaline, 8 parts of black magnetite, 3 parts of white jade, 3 parts of chestnut carbon powder, 0.01 part of graphite powder, and 0.01 part of citric acid powder and 63 parts of cement, and its preparation method comprises the steps:
[0033] (1) pulverize black tourmaline, black magnetite and white jade to 400 meshes, 140 meshes and 250 meshes through mechanical ball milling respectively, to obtain the crushed stone powder of tertiary particle size: black tourmaline powder, black magnetite powder and white jade powder;
[0034] (2) get chestnut twigs and burn to obtain chestnut charcoal, and through crushing to 400 orders, obtain chestnut charcoal powder;
[0035] (3) after mixing the crushed stone powder of step 1 according to the proportion, add 2.5 times the volume of water, and place it at 40 ° C for immersion at a constant temperature for 25 minut...
Embodiment 2
[0040] A wall material for a geomagnetic function room, according to the ratio of parts by mass, including 10 parts of black tourmaline, 10 parts of black magnetite, 5 parts of white jade, 5 parts of chestnut carbon powder, 0.03 part of graphite powder, and 0.005 part of citric acid powder and 65 parts of cement, its preparation method comprises the steps:
[0041] (1) pulverizing black tourmaline, black magnetite and white jade to 450 meshes, 200 meshes and 300 meshes through mechanical ball milling, respectively, to obtain the crushed stone powder of three-grade particle size: black tourmaline powder, black magnetite powder and white jade powder;
[0042] (2) get chestnut twigs and burn to obtain chestnut charcoal, and through crushing to 450 orders, obtain chestnut charcoal powder;
[0043] (3) After mixing the crushed stone powder in step 1 according to the proportion, add 2 times the volume of water, after stirring at a speed of 100 r / min for 10 minutes, place it at 30 ° ...
Embodiment 3
[0048]A wall material for a geomagnetic function room, according to the ratio of parts by mass, including 9 parts of black tourmaline, 9 parts of black magnetite, 4 parts of white jade, 4 parts of chestnut carbon powder, 0.02 part of graphite powder, and 0.008 part of citric acid powder and 64 parts of cement, its preparation method comprises the steps:
[0049] (1) pulverize black tourmaline, black magnetite and white jade to 400 meshes, 200 meshes and 300 meshes through mechanical ball milling, respectively, to obtain crushed stone powders with three-grade particle size: black tourmaline powder, black magnetite powder and white jade powder;
[0050] (2) get chestnut twigs and burn to obtain chestnut charcoal, and through crushing to 400 orders, obtain chestnut charcoal powder;
[0051] (3) After mixing the crushed stone powder in step 1 according to the proportion, add 2 times the volume of water, and after stirring at a speed of 120 r / min for 8 minutes, place it at 35 ° C a...