Waste leather renovating method
A leather and waste technology, applied in the field of refurbishment of waste leather, can solve the problems of not being able to get rid of the old and aging feeling, high toxicity, high labor intensity, etc., and achieve the effects of low toxicity in the production environment, recovery of sensory properties, and high production efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0041] A method for refurbishing waste and old leather, comprising a treatment agent deployment process, a leather pretreatment process and a leather renewing process, specifically:
[0042] Ⅰ. Preparation process of treatment agent
[0043] Calculated in parts by weight, mix 70 parts of water, 5 parts of low-carbon alcohol, 2 parts of low-carbon ether and 0.5 part of ammonia water, mix well and cool to room temperature to prepare the treatment agent; the water used is warm water with a temperature of 30±2°C .
[0044] Ⅱ. Leather pretreatment process
[0045] First put 1000kg of waste leather in a stainless steel container, pass hot air at 85°C into the stainless steel container, keep the relative humidity at 100%, and let it stand for 20 minutes;
[0046] Then, after cooling the heat-treated leather to normal temperature, transfer it to a drum with constant temperature and humidity. At the same time, add 10kg of warm water at 60±2°C and 5kg of the treatment agent formulated...
Embodiment 2
[0051]A method for refurbishing waste and old leather, comprising a treatment agent deployment process, a leather pretreatment process and a leather renewing process, specifically:
[0052] Ⅰ. Preparation process of treatment agent
[0053] Calculated in parts by weight, mix 72 parts of water, 6 parts of low-carbon alcohol, 3 parts of low-carbon ether and 0.6 part of ammonia water, mix well and cool to normal temperature to prepare the treatment agent; the water used is warm water with a temperature of 30±2°C .
[0054] Ⅱ. Leather pretreatment process
[0055] First put 100kg of waste leather in a stainless steel container, pass hot air at 88°C into the stainless steel container, keep the relative humidity at 100%, and let it stand for 25 minutes;
[0056] Then cool the heat-treated leather to normal temperature, transfer it to a drum with constant temperature and humidity, add 25kg of water at 60±2°C and 8kg of the treatment agent prepared in step 1 to the drum, and turn on...
Embodiment 3
[0061] A method for refurbishing waste and old leather, comprising a treatment agent deployment process, a leather pretreatment process and a leather renewing process, specifically:
[0062] Ⅰ. Preparation process of treatment agent
[0063] Calculated by weight, mix 72 parts of water, 6 parts of low-carbon alcohol, 3 parts of low-carbon ether and 0.7 part of ammonia water, and mix well to prepare the treatment agent; the water used is warm water with a temperature of 30±2°C.
[0064] Ⅱ. Leather pretreatment process
[0065] First put 1000kg of waste leather in a stainless steel container, pass hot air at 90°C into the stainless steel container, keep the relative humidity at 100%, and let it stand for 24 minutes;
[0066] Then cool the heat-treated leather to room temperature, transfer it to a drum with constant temperature and humidity, add 30kg of warm water at 60±2°C and 10kg of the treatment agent prepared in step 1 to the drum, and turn on the drum for 4 hours Finally, ...