An anti-allergic, baby-friendly technology, applied in the field of building decoration materials, can solve the problems of prone to allergies, discoloration of the paint film surface, and susceptibility to bacterial infection, etc., to relieve and treat dry skin, high antibacterial efficiency, and relieve skin redness and swelling Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
specific Embodiment approach
[0035] An antibacterial and hypoallergenic coating for babies, which is prepared from the following raw materials according to the following mass proportions through the following steps:
[0036] (1) Add 15-20 parts of water into the dispersing tank, add 0.2-0.5 parts of hydroxyethyl cellulose and 0.1-0.3 parts of water-based multifunctional additives in sequence at a speed of ≤550r / min, and disperse for 1min-3min;
[0037] (2) After increasing the speed to 800-1000r / min, add 0.5-1.0 parts of water-based dispersant, 0.1-0.2 parts of water-based wetting agent, 0.2-0.6 parts of water-based defoamer, 8-12 parts of titanium dioxide, 5- After 7 parts of kaolin, 8-10 parts of talcum powder and 6-8 parts of calcium carbonate, increase the speed again to 1800-2000r / min and disperse for 15min-20min, then check whether the fineness is ≤60μm, if the fineness is ≤60μm, continue Execute step (3);
[0038] (3) Reduce the rotation speed to 1000-1200r / min, add 43-45 parts of styrene-acrylic ...
Embodiment 1
[0041] Embodiment 1 (best embodiment)
[0042] An antibacterial and hypoallergenic coating for babies, which is prepared from the following raw materials according to the following mass proportions through the following steps:
[0043] (1) Add 16 parts of water into the dispersing tank, add 0.4 parts of hydroxyethyl cellulose and 0.3 parts of water-based multifunctional additives at a speed of 400r / min, and disperse for 3 minutes;
[0044] (2) After increasing the rotation speed to 800r / min, add 0.6 parts of water-based dispersant, 0.1 part of water-based wetting agent, 0.5 parts of water-based defoamer, 12 parts of titanium dioxide, 5 parts of kaolin, 9 parts of talcum powder and 8 parts of carbonic acid After calcium, increase the speed again to 2000r / min and disperse for 18 minutes, then check whether the fineness is ≤60 μm, and if the fineness is ≤60 μm, continue to step (3);
[0045] (3) Reduce the rotation speed to 1200r / min, add 44 parts of styrene-acrylic emulsion, 2....
Embodiment 2
[0047] An antibacterial and hypoallergenic coating for babies, which is prepared from the following raw materials according to the following mass proportions through the following steps:
[0048] (1) Add 19 parts of water into the dispersing tank, add 0.5 parts of hydroxyethyl cellulose and 0.28 parts of water-based multifunctional additives successively at a speed of 350r / min, and disperse for 1 min;
[0049] (2) After increasing the rotation speed to 800r / min, add 1 part of water-based dispersant, 0.1 part of water-based wetting agent, 0.2 part of water-based defoamer, 8.1 parts of titanium dioxide, 5 parts of kaolin, 10 parts of talcum powder and 6 parts of carbonic acid After calcium, increase the speed again to 2000r / min and disperse for 15 minutes, then check whether the fineness is ≤60 μm, and if the fineness is ≤60 μm, continue to step (3);
[0050] (3) Reduce the rotation speed to 1000r / min, add 45 parts of styrene-acrylic emulsion, 3 parts of film-forming aids, 0.8 p...