A laser selective melting and brittle alloy technology, which is applied in the direction of process efficiency improvement, additive manufacturing, and energy efficiency improvement, can solve the problems of poor plasticity of brittle alloys, and achieve the effect of avoiding waste and increasing the scope of application

Active Publication Date: 2021-01-05
HUAZHONG UNIV OF SCI & TECH
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] Aiming at the problem that the poor plasticity of brittle alloys limits its application, the present invention is based on the layered size effect and uses laser selective melting technology to manufacture brittle alloys and a tough alloy layer by layer. By adjusting the brittle alloy and toughness The thickness of the metal sheet can realize the controllable fracture form of the material, thereby overcoming the limitation of poor plasticity of brittle alloys and improving the application range of brittle alloys

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A laser selective melting method for brittle alloys with lamellar size effect
  • A laser selective melting method for brittle alloys with lamellar size effect
  • A laser selective melting method for brittle alloys with lamellar size effect

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0024] The invention provides a preparation method of a brittle alloy with layered size effect by laser selective melting technology, the method comprising the following steps:

[0025] (1) sieving the brittle alloy powder and the ductile alloy powder to obtain powder raw materials of suitable particle size in normal distribution;

[0026] (2) Put the sieved raw material into an oven to dry, remove the moisture therein, prevent the sample from being polluted during the printing process, and prepare for forming;

[0027] (3) Put the dried ductile alloy powder 7 into the raw material chamber 1, start the equipment, and inject argon gas to remove oxygen in the forming space to avoid oxidation of the formed part. The heater 3 is raised to a certain temperature to preheat the ductile alloy powder;

[0028] (4) spread the preheated ductile alloy powder in the forming cavity 2 with the powder spreading roller 4, and the excess powder falls into the spare cavity 6, and then under the...

Embodiment 1

[0041] figure 2 It is a flow chart of a TiAl alloy laser selective melting technology preparation method with layered size effect according to an embodiment of the present invention. The first is a schematic diagram of raw material loading for laser selective melting equipment, the second is a schematic diagram of the process of ductile alloy laser selective melting, and the third is a schematic diagram of replacing the raw material with TiAl alloy powder after a layer of ductile alloy is manufactured. The fourth is a schematic diagram for completing a manufacturing cycle. Such as figure 2 Shown, a kind of TiAl alloy laser selective area melting technology preparation method with layered size effect, this method comprises the following steps:

[0042] (1) Raw material screening: TiAl alloy powder and ductile alloy powder are sieved with 270 mesh and 800 mesh sieves respectively, and the 270 mesh sieve and 800 mesh sieve are taken to obtain powders with suitable particle si...

Embodiment 2

[0050] A preparation method of a TiAl alloy with layered size effect by laser selective melting technology in the embodiment of the present invention is used to prepare the Inconel 718 / TiAl alloy with layered size effect by using the laser selective melting technology of the present invention. The specific steps are as follows:

[0051] (1) First, sieve TiAl alloy powder and Inconel 718 powder with 270-mesh and 800-mesh sieves respectively, and take 270-mesh under-sieve and 800-mesh sieve to obtain raw material powder with particle size distribution between 15 and 53 μm ;

[0052] (2) Put the sieved Inconel 718 and TiAl alloy raw materials into an oven for drying, and place them at 80° C. for 5 hours to remove the moisture therein;

[0053] (3) Inconel 718 after drying is packed in raw material cavity 1, at this moment figure 2 The 7 in it is Inconel 718, and then argon gas is introduced to reduce the oxygen content in the forming chamber to below 0.4% to avoid oxidation dur...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
thicknessaaaaaaaaaa
particle diameteraaaaaaaaaa
Login to View More

Abstract

The invention relates to a laser selective melting preparation method of a brittle alloy with layered size effect, and belongs to the field of advanced manufacturing technology. Place the ductile alloy powder in the raw material cylinder of the laser selective melting device, and after preheating, scan the ductile alloy powder to form a tough alloy layer with a certain thickness; the elongation of the ductile alloy material should be greater than or equal to 5%; The ductile alloy powder in the raw material cylinder is replaced with brittle alloy powder, and after preheating, the brittle alloy powder is formed by laser scanning; the elongation of the brittle alloy material is less than 5%; the ductile alloy layer and the brittle alloy layer are alternately prepared Finally, the last layer is a ductile alloy layer, that is, a layered TiAl alloy with controllable properties is obtained. The invention uses the laser selective melting technology to compound the brittle alloy and another alloy with better toughness in the form of lamellar, and manufactures the brittle alloy composite material with more excellent performance based on the lamellar size effect.

Description

technical field [0001] The invention belongs to the field of advanced manufacturing technology, and in particular relates to a method for preparing a brittle alloy by laser selective melting with layered size effect. Background technique [0002] Laser selective melting technology (SLM) is a kind of additive manufacturing technology. Through layer-by-layer manufacturing and accumulation, the required components can be finally obtained. In theory, any complex shape can be formed, and the unformed raw materials can be reused during the manufacturing process. , no material waste, approaching or achieving near-net shape. Compared with the traditional manufacturing method, in the selective laser melting manufacturing process, the sample can be melted and solidified rapidly in the micro-area of ​​the laser action. At a very high cooling rate, the alloy often has finer grains, which can improve The strength of formed parts is even comparable to that of forgings. Moreover, laser f...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): B22F3/105B22F7/02B33Y10/00
CPCB22F7/02B33Y10/00B22F10/00B22F10/36B22F12/13B22F10/28Y02P10/25
Inventor宋波范军翔李继展史玉升
OwnerHUAZHONG UNIV OF SCI & TECH