A composition and coating technology, applied in the direction of anti-corrosion coatings, alkali metal silicate coatings, etc., can solve the problems of ecological environment imbalance, variation reaction, loss of preservatives into water sources, etc., to reduce harmful gases in the air and anti-corrosion performance Excellent, good bactericidal effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] In the present embodiment, the proportions of each component of the coating are shown in Table 2 below:
[0031] Table 2 Concrete component one of coating composition
[0032] components
Accounting for the total mass percentage of the composition (%)
Deionized water
36
[0033] Hydrophobic silicon additive
0.1
Cationic quaternary ammonium salt
0.8
D
0.1
18
0.35
Potassium silicate solution
35
Elastic Acrylic Emulsion
5
opaque polymer
2
Hydrophobic Modified Polyurethane Thickener
0.15
[0034] The concrete preparation process step of this example is:
[0035] (a) Pre-mixing: first weigh the raw materials according to the formula ratio, add 12 parts of deionized water, 0.1 part of hydrophobic silicon additive, 0.1 part of wetting agent, and 0.8 part of cationic quate...
Embodiment 2
[0041] In the present embodiment, the proportions of each component of the coating are shown in Table 3 below:
[0042] Table 3 Coating Composition Concrete Component Two
[0043] components
Accounting for the total mass percentage of the composition (%)
Deionized water
43.2
Hydrophobic silicon additive
0.3
dispersion stabilizer
0.6
D
0.2
15
0.35
Potassium silicate solution
28.5
Elastic Acrylic Emulsion
9
opaque polymer
3
Hydrophobic Modified Polyurethane Thickener
0.3
[0044] The concrete preparation process step of this example is:
[0045] (a) Pre-mixing: first weigh the raw materials according to the formula ratio, add 12 parts of deionized water, 0.3 parts of hydrophobic silicon additives, 0.2 parts of wetting agent, and 0.6 parts of cationic quaternary ammonium salt dispers...
Embodiment 3
[0051] In the present embodiment, the proportions of each component of the coating are shown in Table 4 below:
[0052] Table 4 Coating Composition Concrete Component Three
[0053] components
Accounting for the total mass percentage of the composition (%)
Deionized water
47.9
Hydrophobic silicon additive
0.5
dispersion stabilizer
0.5
D
0.3
9
0.35
Potassium silicate solution
20
Elastic Acrylic Emulsion
15
opaque polymer
4
Hydrophobic Modified Polyurethane Thickener
0.45
[0054] The concrete preparation process step of this example is:
[0055] (a) Pre-mixing: first weigh the raw materials according to the formula ratio, add 12 parts of deionized water, 0.5 parts of hydrophobic silicon additives, 0.3 parts of wetting agent, and 0.5 parts of cationic quaternary ammonium salt dispersi...
PUM
Property | Measurement | Unit |
---|---|---|
modulus | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com