Expanded and vitrified small ball wall self-insulation system
A technology of expanding vitrified microbeads and self-insulation, applied in insulation, walls, solid waste management, etc., to achieve the effects of low water absorption, good flexibility and crack resistance, and high fire protection rating
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
example 1
[0038] Expansion vitrified microbead thermal insulation blocks: 19 parts of cement, 15 parts of fly ash, 6 parts of expanded vitrified microbeads, 5 parts of slag, 4 parts of quartz sand, 16 parts of rice seeds, and 35 parts of water.
[0039] Masonry mortar with expanded vitrified beads: 30 parts of cement, 20 parts of quartz sand, 9 parts of expanded vitrified beads, 0.27 parts of redispersible rubber powder, 0.2 parts of enhanced anti-cracking agent, 0.03 parts of air-entraining agent, water retention 0.5 parts of agent, 40 parts of water.
[0040] Expansion vitrified microbead thermal insulation template: 48 parts of cement, 15 parts of expanded vitrified microbeads, 0.21 parts of redispersible rubber powder, 0.4 parts of anti-cracking enhancer, 0.04 parts of air-entraining agent, 0.25 parts of water-retaining agent, water reducing 0.1 parts of enhancer, 36 parts of water.
example 2
[0042] Expansion vitrified microbead insulation blocks: 20 parts of cement, 14 parts of fly ash, 6 parts of expanded vitrified microbeads, 6 parts of slag, 3 parts of quartz sand, 16 parts of rice seeds, and 35 parts of water.
[0043] Masonry mortar with expanded vitrified beads: 29 parts of cement, 19 parts of quartz sand, 10 parts of expanded vitrified beads, 0.27 parts of redispersible rubber powder, 0.2 parts of enhanced anti-cracking agent, 0.03 parts of air-entraining agent, water retention 0.5 part of agent, 39 parts of water.
[0044]Expansion vitrified microbead thermal insulation template: 47 parts of cement, 16 parts of expanded vitrified microbeads, 0.16 parts of redispersible rubber powder, 0.5 parts of anti-cracking enhancer, 0.04 parts of air-entraining agent, 0.2 parts of water-retaining agent, water reducing 0.1 parts of enhancer, 36 parts of water.
example 3
[0046] Expansion vitrified microbead thermal insulation blocks: 21 parts of cement, 14 parts of fly ash, 6 parts of expanded vitrified microbeads, 4 parts of slag, 3 parts of quartz sand, 17 parts of rice seeds, and 35 parts of water.
[0047] Masonry mortar with expanded vitrified microbeads: 28 parts of cement, 21 parts of quartz sand, 10 parts of expanded vitrified microbeads, 0.3 parts of redispersible rubber powder, 0.2 parts of enhanced anti-cracking agent, 0.03 parts of air-entraining agent, water retention agent 0.47 parts, 40 parts of water.
[0048] Expansion vitrified microbead thermal insulation template: 50 parts of cement, 14 parts of expanded vitrified microbeads, 0.23 parts of redispersible rubber powder, 0.4 parts of anti-cracking enhancer, 0.04 parts of air-entraining agent, 0.23 parts of water-retaining agent, water reducing 0.1 part of enhancer, 35 parts of water.
[0049] Table 1
[0050]
[0051]
[0052] Table 2
[0053]
[0054] table 3
[...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com