Mercury-free full-protection paste type zinc-manganese battery
A zinc-manganese battery and anti-paste technology, which is applied to dry batteries, battery pack components, circuits, etc., can solve problems such as implementation difficulties and unsatisfactory battery electrical performance, and achieve enhanced corrosion inhibition effect, good corrosion inhibition effect, and cost. low effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] R20S mercury-free full anti-paste zinc-manganese battery electrolyte formula contains ZnCl per liter of electrolyte 2 15.5%, NH 4 Cl 20%, the balance is water; the ratio of flour and starch in each liter of electro-liquid is 3:7, and the slurry contains 8% flour, 18.5% starch, 2% polyacrylamide, 25% ammonium chloride, Zinc 14%, the balance is water. In addition, add mercury-free corrosion inhibitors in the slurry: the weight percentage of cetyltrimethylammonium bromide (CTAB) in the slurry is 0.03%, the weight percentage of sodium dodecylbenzenesulfonate (SDBS) in the slurry 0.04%, bismuth trichloride (BiCl 3 ) is 0.03% by weight in the slurry. Through stirring, filtering, and controlling the viscosity, make a mercury-free slurry, input it into the production line, inject it into the zinc cylinder, and form an isolation layer between the zinc cylinder and the battery core, and make the slurry mature and solidify through the gelatinization process without mercury cor...
Embodiment 2
[0024] The electrolyte formula and slurry formula are the same as in Example 1, except that the weight percentage of mercury-free corrosion inhibitor cetyltrimethylammonium bromide (CTAB) added to the slurry is 0.025%, dodecylbenzenesulfonic acid The weight percentage of sodium (SDBS) is 0.035%, bismuth trichloride (BiCl 3 ) is 0.05% by weight.
Embodiment 3
[0026] The electrolyte formula and slurry formula are the same as in Example 1, except that the weight percentage of mercury-free corrosion inhibitor cetyltrimethylammonium bromide (CTAB) added to the slurry is 0.025%, dodecylbenzenesulfonic acid The weight percentage of sodium (SDBS) is 0.035%, bismuth trichloride (BiCl 3 ) is 0.04% by weight.
[0027] The battery production process of the above three embodiments is the same as the traditional full anti-paste zinc-manganese battery production process. The open-circuit voltage of the battery produced according to the corrosion inhibitor ratio of the three examples is 1.65V-1.725V, the short-circuit current: ≥6.0A, and the electrical properties all meet the requirements of the GB8897.2-2005 standard.
[0028] Through the battery test, observe the corrosion situation of the inner surface of the new battery, the zinc cylinder stored for half a year and one year, it is shown that the three corrosion inhibitors of the present inve...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 