[0024] 1. Formula ratio (by weight)
[0025] Configure 1000kg of non-toxic and harmless elastic emulsion, and its raw material ratio (kg) is:
[0026] Dispersant 8045 2
[0027] Defoamer N×2 1
[0028] Dibutyl ester 10
[0029] Heavy calcium 600 mesh 200
[0030] Wollastonite powder 1250 mesh 100
[0031] Elastic emulsion VAE718 500
[0032] Fungicide 3
[0033] edible strong flour 2
[0034] Thickener TT935 2
[0035] water 180.
[0036] 2, preparation method, comprises the steps:
[0037] (1) Add water, dispersant, defoamer and plasticizer into the mixing tank in sequence, and stir for 3 minutes at a speed of 400 rpm;
[0038] (2) Add elastic emulsion and bactericide, and continue stirring for 3 minutes;
[0039] (3) Add heavy calcium and wollastonite powder in sequence, and stir for 15 minutes at a speed of 450 rpm. The speed should be as high as possible under the premise of not generating vortex wrapping air, and then;
[0040] (4) Reduce the rotation speed to...
Embodiment 2
[0044] 1. Formula ratio (by weight)
[0045] Configure 1000kg of non-toxic and harmless elastic emulsion, and its raw material ratio (kg) is:
[0046] Dispersant 8045 2
[0047] Defoamer N×2 1
[0048] Dibutyl ester 10
[0049] Heavy calcium 400 mesh 200
[0050] Wollastonite powder 800 mesh 100
[0051] Elastic emulsion VAE718 500
[0052] Fungicide 3
[0053] edible strong flour 2
[0054] Thickener TT935 2
[0055] water 180.
[0056] 2, preparation method, comprises the steps:
[0057] (1) Add water, dispersant, defoamer and plasticizer into the mixing tank in sequence, and stir for 3 minutes at a speed of 400 rpm;
[0058] (2) Add elastic emulsion and bactericide, and continue stirring for 3 minutes;
[0059] (3) Add heavy calcium and wollastonite powder in sequence, and stir for 15 minutes at a speed of 450 rpm. The speed should be as high as possible under the premise of not generating vortex wrapping air, and then;
[0060] (4) Reduce the rotation speed to ...
Embodiment 3
[0063] 1. Formula ratio (by weight)
[0064] Configure 1000kg of non-toxic and harmless elastic emulsion, and its raw material ratio (kg) is:
[0065] Dispersant 8045 2
[0066] Defoamer N×2 1
[0067] Dibutyl ester 10
[0068] Heavy calcium 600 mesh 190
[0069] Rutile titanium dioxide 10
[0070] Wollastonite powder 1250 mesh 100
[0071] Elastic emulsion VAE718 500
[0072] Fungicide 3
[0073] edible strong flour 2
[0074] Thickener TT935 2
[0075] water 180.
[0076] 2, preparation method, comprises the steps:
[0077] (1) Add water, dispersant, defoamer and plasticizer into the mixing tank in sequence, and stir for 3 minutes at a speed of 400 rpm;
[0078] (2) Add elastic emulsion and bactericide, and continue stirring for 3 minutes;
[0079] (3) Add heavy calcium and wollastonite powder in sequence, and stir for 20 minutes at a speed of 400 rpm. The speed should be as high as possible under the premise of not generating vortex wrapping air, and then;
[008...
PUM
Property | Measurement | Unit |
---|---|---|
Tensile strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
![application no application](https://static-eureka.patsnap.com/ssr/23.2.0/_nuxt/application.06fe782c.png)
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com