Water-based paint mist coagulant, and preparation method and application thereof

A technology of paint mist coagulant and water-based paint, which is applied in chemical instruments and methods, water/sewage treatment, water/sludge/sewage treatment, etc. Floating, incomplete detackification of water-based paint and other problems, to achieve the effect of easy control of production conditions, low cost and high yield

Pending Publication Date: 2020-08-28
深圳市众望丽华实业有限公司
View PDF5 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0006] In the above-mentioned technology, the paint mist coagulant is a double-dose type, that is, the anti-tack agent is used in conjunction with the flocculant, but the inventor of the present application found that the above-mentioned technology has at least the following technical problems in the process of realizing the embodiment of the application: (1) The flocculation speed is slow and the treatment efficiency is low; (2) The decolorization effect is poor, and the decolorization rate of the wastewater containing aqueous paint mist is low; (3) The paint slag floats completely, and the paint slag will sink after the final wastewater quality is clear. Unable to float for a long time, the water quality of the wastewater cannot be kept clear and transparent for a long time, resulting in the turbidity of the wastewater not meeting the standard; (4) The anti-viscosity agent and flocculant itself contain a pH regulator, or the pH of the wastewater needs to be adjusted externally when using the product, and the operation is complicated and cumbersome (5) The detackification and flocculation effects need to be further improved, the detackification of water-based paint is not complete, and the particles of floating paint slag are small, easy to disperse, and difficult to salvage

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0047] In the second aspect, the preparation method of the water-based paint mist coagulant in the first aspect is provided, comprising the steps:

[0048] Preparation of anti-viscosity agent A: add inorganic metal salt into water, stir evenly, then add cationic monomer, stir evenly, and set aside for later use; more specifically, in the preparation of anti-viscosity agent A, at 30-45°C, Add the inorganic metal salt into the water, stir for 0.8-1.2 hours to completely dissolve it, then add the cationic monomer, stir for 0.8-1.2 hours to completely dissolve it, and place it for 4 hours before use.

[0049] Preparation of flocculant B: Add one of xanthan gum, Wenlun gum, polyacrylamide, and lignin while stirring in water, and then add xanthan gum, Wenlun gum, polyacrylamide, and Another one of lignin, stirred to dissolve completely;

[0050] Pack the anti-tack agent A and flocculant B separately.

[0051] The preparation of the water-based paint mist coagulant by the invention...

Embodiment 1

[0059] A kind of water-based paint mist coagulant, which is composed of anti-tack agent A and flocculant B; said anti-tack agent A is formulated from the following raw materials in weight percentage: 15% of inorganic metal salt, 1.5% of cationic monomer, The balance is water; the inorganic metal salt is polyaluminum ferric chloride; the cationic monomer is methacryloyloxyethyltrimethylammonium chloride.

[0060] The active ingredients of the flocculant B are xanthan gum and polyacrylamide, the molecular weight of the polyacrylamide is 12 million, the mass percentage of xanthan gum in the flocculant B is 0.5%, and the mass percentage of the flocculant B is The mass percentage of polyacrylamide is 0.5%.

[0061] The preparation method of above-mentioned water-based paint mist coagulant, the steps are as follows:

[0062] Preparation of anti-viscosity agent A: Add inorganic metal salts into water at 40°C, stir for 1 hour to dissolve completely, then add cationic monomer, stir fo...

Embodiment 2

[0066] A water-based paint mist coagulant, which is composed of a tack-free agent A and a flocculant B; the tack-breaker A is formulated from the following raw materials in weight percentage: 5% inorganic metal salt, 0.5% cationic monomer, The balance is water; the inorganic metal salt is aluminum chloride hydroxy; the cationic monomer is dimethyl diallyl ammonium chloride.

[0067] The active ingredients of the flocculant B are xanthan gum and Wenlun gum, and the mass percentage of the active ingredients in the flocculant B is 0.2%.

[0068] The preparation method of above-mentioned water-based paint mist coagulant, the steps are as follows:

[0069] Preparation of anti-viscosity agent A: Add inorganic metal salt into water at 30°C, stir for 1.2 hours to dissolve completely, then add cationic monomer, stir for 1.2 hours to dissolve completely, leave it for 4 hours for later use.

[0070] Preparation of flocculant B: at room temperature, add xanthan gum while stirring in wate...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a water-based paint mist coagulant, and a preparation method and an application thereof. The water-based paint mist coagulant is composed of an anti-sticking agent A and a flocculating agent B. The effective components of the anti-sticking agent A are an inorganic metal salt and a cationic monomer, the mass ratio of the inorganic metal salt to the cationic monomer is (8-12): 1, and the mass percentage of the effective components in the anti-sticking agent A is 5-40%. The effective components of the flocculating agent B are two of xanthan gum, welan gum, polyacrylamide and lignin, and the mass percentage of the effective components in the flocculating agent B is 0.1-3%. Through the combination and proportioning, the flocculation is fast; the decolorization rate is high; paint slag is not easy to sink and can float upwards for a long time, so that the clarity of the wastewater can be ensured; the water-based paint mist coagulant has good viscosity reduction and coagulation effects on water-based paints, the water-based paints can be thoroughly debonded, floating paint slag can be bonded into large blocks, fishing is easy, and pH does not need to be adjusted.

Description

technical field [0001] The invention relates to the technical field of paint-containing wastewater treatment, in particular to a water-based paint mist coagulant and its preparation method and application. Background technique [0002] When using oil-based paint for painting, because the oil-based paint contains toxic benzene compounds and other substances, a large amount of harmful gases will be generated during the painting process, which will damage human health, and the discharged wastewater will also seriously endanger the environment. As the country begins to pay attention to the protection of the ecological environment, environmental protection requirements are becoming more and more stringent. Water-based paint uses water as a diluent, which does not use organic solvents, has good environmental protection characteristics, is non-flammable, does not contain carcinogens, and is less harmful to humans. Favored by more and more painting users, the use of water-based pain...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): C02F1/52C02F1/54C02F1/56
CPCC02F1/5263C02F1/5245C02F1/54C02F1/56
Inventor 任嘉孙健
Owner 深圳市众望丽华实业有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products