Acicular ferrite type high-strength steel bar and preparation method thereof

A technology of acicular ferrite and high-strength steel bars is applied in the direction of improving process efficiency, which can solve the problems of affecting the plasticity index and time-efficiency performance of steel bars, unfavorable to the promotion of large-scale industrial production, and subcutaneous bubbles of continuous casting billets, and achieves secondary hardening. The effect is obvious, the pearlite structure is refined, and the hardenability is improved

Pending Publication Date: 2022-02-08
安徽吾兴新材料有限公司
View PDF7 Cites 5 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

There are the following deficiencies: tempering induction heater heating, grain stabilization treatment, etc., the process is complicated, which is not conducive to the promotion of large-scale industrial production
The disadvantages are: the N content is too high, it is easy to cause defects such as subcutaneous air bubbles in the continuous casting slab, and it will affect the plasticity index and aging performance of the steel bar

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Acicular ferrite type high-strength steel bar and preparation method thereof
  • Acicular ferrite type high-strength steel bar and preparation method thereof
  • Acicular ferrite type high-strength steel bar and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0036] This embodiment provides an acicular ferrite high-strength steel bar and a preparation method thereof, comprising the following steps:

[0037] S1, 85% molten iron + 15% scrap steel, the composition of the final molten steel, 0.06% C, and the temperature of the final molten steel is 1650°C;

[0038] S2. The time from the ladle entering the LF furnace refining station to the completion of feeding is 7 minutes. The temperature of the molten steel in the ladle is 1550°C. The temperature of the electrode is raised for 15 minutes. Add wollastonite 0kg / t molten steel and lime 6.5kg / t molten steel, and the composition of the molten steel reaches The above target value, the temperature is 1550°C;

[0039] S3. The pouring time of molten steel from the LF furnace refining station to the continuous casting platform is 10 minutes, the ladle is opened and poured for 25 seconds, and the open pouring time is 10 seconds when the tundish is replaced with a sizing nozzle, and the cooling...

Embodiment 2

[0042] This embodiment provides an acicular ferrite high-strength steel bar and a preparation method thereof, comprising the following steps:

[0043] S1, 85% molten iron + 15% scrap steel, the component of molten steel at the end point, 0.07% C, and the temperature of molten steel at the end point is 1665°C;

[0044] S2. The time from the ladle entering the LF furnace refining station to the completion of feeding is 6 minutes. The temperature of molten steel in the ladle is 1560°C, and the heating time is 14 minutes. Add 2.75kg / t of wollastonite and 4.4kg / t of lime to reach the above-mentioned composition Target value, temperature 1560°C;

[0045] S3. The pouring time of molten steel from the LF furnace refining station to the continuous casting platform is 9 minutes, the ladle is opened and poured for 23 seconds, the tundish is replaced with a sizing nozzle and the pouring time is opened for 9 seconds, the cooling water flow rate of the crystallizer: 115m 3 / h, the specific...

Embodiment 3

[0048] This embodiment provides an acicular ferrite high-strength steel bar and a preparation method thereof, comprising the following steps:

[0049] S1, 85% molten iron + 15% scrap steel, final molten steel composition, 0.08% C, final molten steel temperature 1680°C;

[0050] S2. The time from the ladle entering the LF furnace refining station to the completion of feeding is 5 minutes. The temperature of the molten steel in the ladle is 1570°C. For 13 minutes, add wollastonite 5.5kg / t molten steel and lime 2.3kg / t molten steel, and the composition of the molten steel reaches the above target value, temperature 1570℃;

[0051] S3. The pouring time of molten steel from the refining station of the LF furnace to the continuous casting table is 8 minutes, the pouring time of the ladle is 21 seconds, the pouring time of the tundish is 8 seconds when the sizing nozzle is changed, and the cooling water flow rate of the crystallizer: 130m 3 / h, the cooling ratio of water in the seco...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
yield strengthaaaaaaaaaa
yield strengthaaaaaaaaaa
tensile strengthaaaaaaaaaa
Login to view more

Abstract

The invention belongs to the technical field of hot-rolled ribbed steel bars for reinforced concrete structures, and particularly relates to an acicular ferrite type high-strength steel bar and a preparation method thereof. Steel in the steel bar comprises the following chemical components in percentage by weight: 0.25 to 0.35 percent of C, 0.40 to 0.80 percent of Si, 1.40 to 1.80 percent of Mn, less than or equal to 0.030 percent of P, less than or equal to 0.030 percent of S, 0.02 to 0.04 percent of Nb, 0.09 to 0.15 percent of V, 0.15 to 0.45 percent of Cr, 0.010 to 0.019 percent of N and the balance of Fe and inevitable impurity elements. Under the condition of existing process equipment of a production plant, the acicular ferrite type high-strength steel bar is prepared by adopting a high C, Si and Mn component design and a V and Nb combined microalloying mode and combining a rolling self-tempering process, the 700MPa-grade reinforcing steel bar with excellent comprehensive performance is produced on the premise of keeping material ductility, the yield strength of the 700MPa-grade reinforcing steel bar is greater than or equal to 700MPa, the tensile strength is greater than or equal to 830MPa, the percentage elongation after fracture is greater than or equal to 14%, the total elongation under the maximum force is greater than or equal to 9%, the anti-seismic performance is good, and the requirements of high-rise and large-span anti-seismic structures are met.

Description

technical field [0001] The invention belongs to the technical field of hot-rolled ribbed steel bars for concrete, and in particular relates to an acicular ferrite high-strength steel bar and a preparation method thereof. Background technique [0002] Compared with ordinary steel bars, high-strength steel bars have the advantages of high strength, excellent comprehensive performance, energy saving and environmental protection, long service life, and high safety performance. Foreign developed countries have already eliminated steel bars with lower strength levels such as 335MPa. Britain, Germany, Australia, France and other countries have widely used high-strength steel bars with a yield strength of 500MPa. rebar. In recent years, with the introduction of a series of high-strength steel promotion and application policies in my country, the percentage of high-strength steel consumption has increased year by year. At present, domestic HRB500 high-strength steel bars have been ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C21D8/08B22D11/00C22C33/04C22C38/00C22C38/02C22C38/04C22C38/24C22C38/26
CPCC22C33/04C22C38/02C22C38/04C22C38/26C22C38/24C22C38/001B22D11/005C21D8/065C21D8/08Y02P10/20
Inventor 魏滔锴黄华
Owner 安徽吾兴新材料有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products