An inorganic nano and nano silver technology, applied in manufacturing tools, chemical instruments and methods, wood-layered products, etc., can solve problems such as heat resistance, poor durability, increase air pollution sources, and air quality deterioration, and achieve stable performance, Improve indoor air quality and fine particle size
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] (1) Sand the 3mm thick miscellaneous wood plywood to a certain thickness, and use it as the base material for later use.
[0037] (2) Immerse the 0.2mm thick natural red oak decorative veneer in the pre-prepared inorganic nano-silver aqueous solution. The concentration of nano-silver in this solution is 50ppm, and the content of acrylic resin in the solution is 1%. After the decorative veneer is dipped, dry it and set it aside.
[0038] (3) The glue ratio is: adhesive 100kg, flour 20±2kg, inorganic nano-silver aqueous solution 9g, ammonium chloride 1±0.1kg. The adhesive is modified urea-formaldehyde resin glue or phenolic resin glue.
[0039] (4) Paste the impregnated red oak decorative veneer on the glued miscellaneous wood plywood, and the amount of glue on one side is 80g / m 2 .
[0040](5) After veneering, pre-pressing, hot-pressing, post-sanding and other processes are carried out to form an inorganic nano-silver anti-mold, anti-bacterial, healthy red oak decora...
Embodiment 2
[0043] (1) Sand the 5mm thick medium-density fiberboard to a certain thickness, and use it as a base material for later use.
[0044] (2) Immerse the 0.3mm thick white oak reconstituted decorative veneer in the pre-prepared inorganic nano-silver aqueous solution. The concentration of nano-silver in this solution is 100ppm, and the content of acrylic resin in the solution is 6%. Dried after dipping, set aside.
[0045] (3) The glue ratio is: adhesive 100kg, flour 30±2kg, inorganic nano-silver aqueous solution 16g, ammonium chloride 1±0.1kg. The adhesive is modified urea-formaldehyde resin glue or melamine resin glue.
[0046] (4) Paste the impregnated red oak decorative veneer on the glued medium density fiberboard, the amount of glue on one side is 120g / m 2 .
[0047] (5) After veneering, pre-pressing, hot-pressing, post-sanding and other processes are carried out to form inorganic nano-silver anti-mildew, anti-bacterial, healthy white oak recombined decorative veneer. Th...
Embodiment 3
[0050] (1) Sand the 18mm thick particle board to a certain thickness, and use it as a base material.
[0051] (2) Dip the 0.6mm thick red sandalwood dyed decorative veneer in the pre-prepared inorganic nano-silver aqueous solution. The concentration of nano silver in this solution is 150ppm, and the content of acrylic resin in the solution is 10%. Dried after dipping, set aside.
[0052] (3) The glue ratio is: adhesive 100kg, flour 45±2kg, inorganic nano-silver aqueous solution 22g, ammonium chloride 1±0.1kg. The adhesive is modified urea-formaldehyde resin glue or soybean adhesive.
[0053] (4) Paste the impregnated red sandalwood dyed decorative veneer on the glue-coated particle board, and the amount of glue on one side is 150g / m 2 .
[0054] (5) After veneering, pre-pressing, hot-pressing, post-sanding and other processes are carried out to form inorganic nano-silver anti-mildew, anti-bacterial, healthy white oak recombined decorative veneer. The pre-pressing pressure...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com