Artistic coating and preparation method thereof
An art paint and emulsion technology, applied in the direction of coating, can solve the problems of no layering, single color of latex paint, easy discoloration of wallpaper, etc., to achieve the effect of overcoming edge warping and overcoming single color
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
specific Embodiment approach
[0024] A kind of artistic paint, is formulated by following components and ratio of parts by weight:
[0025]
[0026] The emulsion is a water-based polymer resin formed by copolymerizing vinyl acetate and butyl acrylate as main functional monomers.
[0027] A kind of preparation method of art paint, it comprises the following steps carried out in sequence:
[0028] (1) Add 28-34 parts of water into the dispersion tank, and add 0.2-0.3 parts of hydroxyethyl cellulose, 0.15-0.2 parts of bentonite and 0.15-0.2 parts of water-based multifunctional additives in turn under the stirring state of 350-550r / min , stirring for 1min-3min;
[0029] (2) After increasing the speed to 800-1000r / min, add 0.6-0.7 parts of water-based dispersant, 0.1-0.2 parts of water-based wetting agent, 0.4-0.5 parts of water-based defoamer, 3-7 parts of titanium dioxide, 18- After 22 parts of kaolin, 9-15 parts of calcium carbonate, and 2-4 parts of diatomite, increase the speed again to 1800-2000r / min...
Embodiment 1
[0033] Embodiment 1: a kind of artistic paint, is formulated by following component and weight and number ratio:
[0034]
[0035]
[0036] The emulsion is a water-based polymer resin formed by copolymerizing vinyl acetate and butyl acrylate as main functional monomers.
[0037] A kind of preparation method of art paint, it comprises the following steps carried out in sequence:
[0038](1) Add 29 parts of water into the dispersing tank, add 0.2 parts of hydroxyethyl cellulose, 0.2 parts of bentonite and 0.15 parts of water-based multifunctional additives in sequence under stirring at 550r / min, and stir for 1 min;
[0039] (2) After increasing the speed to 1000r / min, add 0.7 parts of water-based dispersant, 0.15 parts of water-based wetting agent, 0.45 parts of water-based defoamer, 5 parts of titanium dioxide, 18 parts of kaolin, 15 parts of calcium carbonate, and 3 parts of silicon After diatomaceous earth, increase the rotation speed to 2000r / min again and disperse at...
Embodiment 2
[0042] Embodiment 2: a kind of artistic paint, is formulated by following component and weight and number ratio:
[0043]
[0044]
[0045] The emulsion is a water-based polymer resin formed by copolymerizing vinyl acetate and butyl acrylate as main functional monomers.
[0046] A kind of preparation method of art paint, it comprises the following steps carried out in sequence:
[0047] (1) Add 34 parts of water into the dispersing tank, add 0.25 parts of hydroxyethyl cellulose, 0.15 parts of bentonite and 0.2 parts of water-based multifunctional additives in sequence under stirring at 350r / min, and stir for 3 minutes;
[0048] (2) After increasing the speed to 800r / min, add 0.6 parts of water-based dispersant, 0.1 part of water-based wetting agent, 0.4 parts of water-based defoamer, 3 parts of titanium dioxide, 20 parts of kaolin, 11 parts of calcium carbonate, and 4 parts of silicon After diatomaceous earth, increase the rotation speed to 1800r / min again and disperse ...
PUM
Property | Measurement | Unit |
---|---|---|
water absorption | aaaaa | aaaaa |
refractive index | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com