A kind of preparation method of calcium carbonate microspheres

A technology of calcium carbonate and microspheres, applied in the direction of calcium carbonate/strontium/barium, medical preparations of non-active ingredients, pharmaceutical formulas, etc., can solve the complex synthesis process of calcium carbonate microspheres, cumbersome calcium carbonate microsphere methods, Problems such as poor conveying capacity, to achieve the effect of low cost, controllable shape and low consumption

Inactive Publication Date: 2018-05-08
SHANGHAI INST OF TECH
View PDF5 Cites 4 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

So far, the method of preparing calcium carbonate microspheres is still relatively cumbersome
Among them, the hydrothermal method is a relatively common method for preparing calcium carbonate microspheres, but the generation rate is relatively low and the preparation cost is relatively high
The synthesis process of calcium carbonate microspheres synthesized by general precipitation method is complicated and the morphology cannot be controlled
At the same time, the directional delivery ability of most drug-loaded materials is poor

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of preparation method of calcium carbonate microspheres
  • A kind of preparation method of calcium carbonate microspheres
  • A kind of preparation method of calcium carbonate microspheres

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0017] A preparation method of calcium carbonate microspheres, the steps are as follows:

[0018] 1. Prepare 50mL 0.1moL·L separately -1 of calcium chloride and sodium carbonate aqueous solution, and then prepare 10 mL of molar mass concentration of 10 mmol L L -1 of sodium dodecyl sulfonate aqueous solution and 5 mL of polyethyleneimine aqueous solution with a mass percentage concentration of 1%.

[0019] 2. Pour the prepared calcium chloride aqueous solution, sodium dodecyl sulfonate aqueous solution and polyethyleneimine aqueous solution into a 250ml three-necked round-bottomed flask; then place the round-bottomed flask in the ultrasonic instrument and set up a stirring device , and mechanically stirred at 800r / min for 0.5 hours.

[0020] 3. The prepared 50mL 0.1moL·L -1 The sodium carbonate aqueous solution was quickly poured into a 250 ml three-necked round-bottomed flask, and stirred at the original stirring speed in a sonicator for 2 hours. Control the temperature a...

Embodiment 2

[0024] A preparation method of calcium carbonate microspheres, the steps are as follows:

[0025] 1. Prepare 50mL 0.05moL·L separately -1 of calcium chloride and sodium carbonate aqueous solution, and then prepare 10 mL of molar concentration of 15 mmol L L -1 of sodium dodecyl sulfonate aqueous solution and 5 mL of polyethyleneimine aqueous solution with a mass percentage concentration of 2%.

[0026] 2. Pour the prepared calcium chloride aqueous solution, sodium dodecyl sulfonate aqueous solution and polyethyleneimine aqueous solution into a 250ml three-necked round-bottomed flask. The round-bottomed flask was then placed in a sonicator, a stirring device was set up, and mechanical stirring was performed at 800 r / min, and the reaction was carried out for 0.5 hour.

[0027] 3. The prepared 50mL 0.05moL·L -1 The sodium carbonate aqueous solution was quickly poured into a 250 ml three-necked round-bottomed flask, and stirred at the original stirring speed in a sonicator for ...

Embodiment 3

[0031] A preparation method of calcium carbonate microspheres, the steps are as follows:

[0032] 1. Prepare 50mL 0.1moL·L -1 of calcium chloride and sodium carbonate aqueous solution, and then prepare 10 mL of molar concentration of 10 mmol L L -1 The sodium dodecyl sulfate aqueous solution and 5mL mass percent concentration of 2% polyacrylamide aqueous solution,

[0033] 2. Pour the calcium chloride aqueous solution, the sodium lauryl sulfate aqueous solution and the polyvinylamide aqueous solution together into a 250ml three-neck round bottom flask. The round-bottomed flask was then placed in a sonicator, a stirring device was set up, and mechanical stirring was performed at 800 r / min, and the reaction was carried out for 0.5 hour.

[0034] 3. The prepared 50mL 0.1moL·L -1 The sodium carbonate aqueous solution was quickly poured into a 250 ml three-necked round-bottomed flask, and stirred at the original stirring speed in a sonicator for 2 hours. Control the temperature...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
Login to View More

Abstract

The invention discloses a preparation method of calcium carbonate microspheres. The present invention first uses cationic polymers and surfactants to form complex ions with calcium ions in calcium chloride solution; then adds sodium carbonate solution into the reactor, and proceeds under the conditions of ultrasonic and mechanical stirring; after the reaction is completed, centrifuge to remove Impurities in the reaction solution, the precipitate is left and washed with deionized water, filtered, and dried to obtain calcium carbonate microspheres loaded with cationic polymers. The particle size of the calcium carbonate microspheres obtained in the present invention is 900-1500nm; under an electron microscope, it can be found that the spherical microspheres have a stable shape.

Description

technical field [0001] The invention relates to the technical field of medical carriers, in particular to a preparation method of calcium carbonate microspheres. Background technique [0002] Calcium carbonate microspheres are a common non-toxic and biocompatible material. In recent years, calcium carbonate microspheres have been used in drug delivery research. [0003] Since calcium carbonate microspheres can be used for drug carrier delivery, people have been looking for a simple method to prepare calcium carbonate microspheres. So far, the method for preparing calcium carbonate microspheres is still cumbersome. Among them, the hydrothermal method is a relatively common method for preparing calcium carbonate microspheres, but the production rate is relatively low and the preparation cost is relatively high. Generally, the synthesis process of calcium carbonate microspheres by precipitation method is complicated and the morphology cannot be controlled. At the same time, ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): A61K47/32A61K47/04C01F11/18
Inventor豆贤东刘维俊刘晴牛志强
OwnerSHANGHAI INST OF TECH