A kind of efflorescence control method of stone paving veneer
A control method and stone technology, which is applied in the field of gardens and landscapes, can solve the problems of efflorescence on the surface and affect the appearance of stone paving and veneer, and achieve the effects of easy mastery of the process, prevention of efflorescence, and simple and easy construction
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of efflorescence control method of stone paving veneer, concrete steps are as follows,
[0019] Base treatment before laying:
[0020] The concrete wall is painted with waterproof paint twice according to the requirements of the design drawings to close the pores of the concrete surface to prevent water penetration; the brick wall should be leveled with 1:2.5 waterproof mortar, which is mixed with 4-6% of cement weight waterproof Powder; After the surface is dry, apply waterproof paint twice to seal it to prevent dampness and water penetration.
[0021] Waterproof sealing treatment of stone before laying:
[0022] (1) Use a temporary drying room to dry the stone, the drying temperature is 70°C, and dry for 50 minutes to analyze the water in the pores of the stone;
[0023] (2) The configuration of waterproof sealing materials is made of low-alkali cement, water, and ferric chloride according to the weight ratio of cement: water: ferric chloride: 1:5:0.03. First...
Embodiment 2
[0037] A kind of efflorescence control method of stone paving veneer, concrete steps are as follows,
[0038] Base treatment before laying:
[0039] The concrete wall is painted with waterproof paint twice according to the requirements of the design drawings to close the pores of the concrete surface to prevent water penetration; the brick wall should be leveled with 1:2.5 waterproof mortar, which is mixed with 4-6% of cement weight waterproof Powder; After the surface is dry, apply waterproof paint twice to seal it to prevent dampness and water penetration.
[0040] Waterproof sealing treatment of stone before laying:
[0041] (1) Soak the stone in hot water above 80°C for 1 hour, and then dry it naturally for 30 hours to promote the volatilization of residual moisture in the pores of the stone;
[0042] (2) The configuration of waterproof sealing materials is made of low-alkali cement, water, and ferric chloride according to the weight ratio of cement: water: ferric chlori...