Camouflage color yarn production method
A production method, yarn technology, applied in the field of camouflage color yarn production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] A processing method of 60S / 2 gray bottom camouflage blue-violet yarn, comprising the following processing steps:
[0028] 1. Raw yarn preparation
[0029] Choose 60S / 2 high-quality cotton yarn.
[0030] 2. Dyeing
[0031] The base color is gray dyed on the domestic hank dyeing machine, and the uniform dyeing is ensured by controlling the amount of dye, saline and alkali, and color fixing time. The concentration is 0.5%-1% (owf), the amount of salt: 20g / L-30g / L, the amount of alkali 10g / L-20g / L, and the time is 45min.
[0032] 3. Spray dyeing, adopting the spray dyeing process of continuous spot spraying
[0033] Put the yarn flat on the dyeing machine table, add blue to the left nozzle of the first row of nozzles, add purple to the two nozzles on the right, control the speed at 0.99m / min~5m / min, Add water to the second row of nozzles, control the vehicle speed at 0.99m / min~5m / min, bloom the original blue and purple dyes, and form a blue-purple pattern with denser bl...
Embodiment 2
[0042] A kind of processing method of 60S / 2 blue ground camouflage navy blue yarn, comprises following processing steps:
[0043] 1. Raw yarn preparation
[0044] Choose 60S / 2 high-quality cotton yarn.
[0045] 2. Dyeing
[0046] The base color blue is dyed on the domestic skein dyeing machine, and the uniform dyeing is ensured by controlling the amount of dye, saline and alkali, and color fixing time. The concentration is 0.5%-1% (owf), the amount of salt: 20g / L-30g / L, the amount of alkali 10g / L-20g / L, and the time is 45min.
[0047] 3. Spray dyeing, adopting the mist jet dyeing process of intermittent spot spraying
[0048] Put the yarn flat on the dyeing machine workbench, perpendicular to the forward direction, spray the dye intermittently, control the liquid volume at 0.1-2ml / time, spray navy blue dye on one of the nozzles on the first row of nozzles, A small amount of scattered navy blue is formed on the surface of the skein, and finally a small amount of uneven blue...
Embodiment 3
[0057] A kind of processing method of camouflage red yarn of 70S / 2 white background, comprises following processing steps:
[0058] 1. Raw yarn preparation
[0059] Choose 70S / 2 high-quality cotton yarn.
[0060] 2. Spray dyeing, spray dyeing process using the spray method at the top of the nozzle
[0061] Put the yarn flat on the dyeing machine table, spray red dye on one of the nozzles in the first row, because the dye spreads upwards, similar to the principle of a fountain, when it falls on the surface of the yarn, it is in the form of mist Scattered, the vehicle speed is controlled at 0.99m / min to 5m / min, forming a camouflage red pattern on a white background.
[0062] 3. Steam
[0063] The spray-dyed yarn is steamed in a steam box at a temperature of 100° C. to 110° C. for 10 minutes to 20 minutes.
[0064] 4. Washing
[0065] 5. Dehydration and drying
[0066] The above-mentioned yarns are put into a rotary drying room for drying, and the yarns are dried at a low t...