[0014] a) softening the tanned sheepskin after tanning and drying at normal temperature;
[0015] b) Carry out retanning treatment on the softened Tan sheepskin, the temperature of the retanning treatment is 30° C., and the time is 12 hours;
[0016] c) Degreasing the retanned sheepskin in the degreasing solution, the degreasing solution contains 0.6mol / L fatty alcohol polyoxyethylene ether and 5g / L washing powder, the degreasing time is 20min, and the temperature is 45°C;
[0017] d) Wash the degreased Tan sheepskin, and carry out a dyeing treatment after washing. The temperature of the first dyeing treatment is 32°C and the time is 35min. The pH of the dyeing slurry in the drum is 3.5, and the drum dyeing slurry contains 0.01g / For the dye of L, the dyeing paste also includes 6.0g / ml of salt, 1ml / L of quaternary ammonium salt formaldehyde-free color fixing agent, and 0.02g / L of acetic acid.
[0018] e) Add formic acid to the drum after the first dyeing treatment to perform...
Embodiment 2
[0023] a) softening the tanned sheepskin after tanning and drying at normal temperature;
[0024] b) Carry out retanning treatment on the softened Tan sheepskin, the temperature of the retanning treatment is 30° C., and the time is 12 hours;
[0025] c) Degreasing the retanned sheepskin in the degreasing solution, the degreasing solution contains 0.7mol / L fatty alcohol polyoxyethylene ether and 7g / L washing powder, the degreasing time is 20min, and the temperature is 40°C;
[0026] d) Wash the Tan sheepskin after the degreasing treatment, and perform a dyeing treatment after washing. The temperature of the first dyeing treatment is 30°C and the time is 35min. The pH of the dyeing slurry in the drum is 4, and the drum dyeing slurry contains 0.008g / For the dye of L, the dyeing paste also includes 6.0g / ml of salt, 1ml / L of quaternary ammonium salt formaldehyde-free color fixing agent, and 0.02g / L of acetic acid.
[0027] e) Add formic acid to the drum after the first dyeing tr...
Embodiment 3
[0032] a) softening the tanned sheepskin after tanning and drying at normal temperature;
[0033] b) Carry out retanning treatment on the softened Tan sheepskin, the temperature of retanning treatment is 32°C, and the time is 10h;
[0034] c) Degreasing the retanned sheepskin in the degreasing solution, the degreasing solution contains 0.6mol / L fatty alcohol polyoxyethylene ether and 7g / L washing powder, the degreasing time is 20min, and the temperature is 40°C;
[0035] d) Wash the degreased Tan sheepskin, and carry out a dyeing treatment after washing. The temperature of the first dyeing treatment is 30°C and the time is 35min. The pH of the dyeing slurry in the drum is 4, and the drum dyeing slurry contains 0.016g / The dye of L, also comprises the salt of 6.0g / ml, the acetic acid of 2ml / L quaternary ammonium salt formaldehyde-free fixing agent, the acetic acid of 0.02g / L in the dyeing paste.
[0036] e) Add formic acid to the drum after the primary dyeing treatment for a ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com