A yellow phosphorus slag and pavement brick technology is applied in the field of autoclaved yellow phosphorus slag pavement bricks and its production, and can solve the problems of low effective utilization rate of yellow phosphorus slag, low strength of ordinary phosphorus slag bricks, unsuitable for pavement masonry, etc. To avoid adverse effects, the production process is easy to control, and the product quality is stable
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] Prepare raw materials according to the batch test volume of 2000 pieces, yellow phosphorus slag powder 3600kg, granular yellow phosphorus slag 1200kg, quicklime powder 180kg, phosphogypsum 1020kg.
[0041] First grind the dried yellow phosphorus slag into powder; then uniformly measure and mix the yellow phosphorus slag powder, granular yellow phosphorus slag, quicklime powder and phosphogypsum in proportion; add water and stir to mix evenly, and control its moisture content at 7% ;Using a brick making machine to make the brick adobe body; and curing with 1.55MPa saturated steam to obtain the finished product.
[0042] Finished product inspection results:
[0043] Compressive strength: 64.7MPa;
[0044] Flexural strength: 20.8MPa;
[0045] Wear resistance: 1.5;
[0046] Water Absorption: 6.9%.
Embodiment 2
[0048] Prepare raw materials according to the batch test volume of 2000 pieces, yellow phosphorus slag powder 1800kg, granular yellow phosphorus slag 3300kg, quicklime powder 130kg, phosphogypsum 770kg.
[0049] First grind the dried yellow phosphorus slag into powder; then uniformly measure and mix the yellow phosphorus slag powder, granular yellow phosphorus slag, quicklime powder and phosphogypsum in proportion; add water and stir to mix evenly, and control its moisture content at 8% ;Using a brick making machine to make the brick adobe; curing with 1.60MPa saturated steam to obtain the finished product.
[0050] Finished product inspection results:
[0051] Compressive strength: 55.3MPa;
[0052] Flexural strength: 17.8MPa;
[0053] Wear resistance: 1.2;
[0054] Water Absorption: 6.9%.
Embodiment 3
[0056] Prepare raw materials according to the batch test volume of 2000 pieces, yellow phosphorus slag powder 2400kg, granular yellow phosphorus slag 3000kg, quicklime powder 100kg, phosphogypsum 500kg.
[0057] First grind the dried yellow phosphorus slag into powder; then uniformly measure and mix the yellow phosphorus slag powder, granular yellow phosphorus slag, quicklime powder and phosphogypsum in proportion; add water and stir to mix evenly, and control its moisture content at 10% ;Using a brick making machine to make the brick adobe body; and curing with 1.55MPa saturated steam to obtain the finished product.
[0058] Finished product inspection results:
[0059] Compressive strength: 53.9MPa;
[0060] Flexural strength: 9.2MPa;
[0061] Wear resistance: 1.3;
[0062] Water absorption: 9.7%.
PUM
Property | Measurement | Unit |
---|---|---|
strength | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
flexural strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com