A low-cost silicon carbide deoxidation method
A silicon carbide, low-cost technology, applied in the field of LF refining, can solve the problems that affect the economic benefits of enterprises, have many inclusions in the billet, increase the economic losses of enterprises, reduce the number of holes and production accidents, and improve the purity of molten steel. , the effect of stabilizing product quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] For Q235B steel, process steps:
[0032] (1) Slag washing is carried out during the tapping process of the converter, and the amount of lime added per ton of steel is 2.4kg; the functions of lime are: ① slagging effect; ② reducing burning loss, and the melt covers the surface of molten steel to prevent excessive oxidation. Through the slag washing in this step, the quality of molten steel can be improved.
[0033] (2) Move the ladle to the refining treatment position, the refining start temperature is 1560°C, the amount of lime added per ton of steel is 4.0kg, the amount of fluorite added per ton of steel is 1.0kg, and the feeding time is 2min. The flow rate is 200NL / min; in the process of adding lime to make slag in this step, there must be a relatively large argon blowing pressure to ensure that the added lime is completely spread on the surface of the ladle, and to ensure that the slag-making material does not accumulate on the side of the feeding hole. White slag p...
Embodiment 2
[0040] For Q345B steel, process steps:
[0041] (1) Slag washing is carried out during the tapping process of the converter, and the amount of lime added per ton of steel is 2.6kg;
[0042] (2) Move the ladle to the refining treatment position, the refining start temperature is 1580°C, the amount of lime added per ton of steel is 6.0kg, the amount of fluorite added per ton of steel is 1.5kg, the feeding time is 3min and the lime time is 1.5min, and the lime is added at a large flow rate. Stirring with argon, the flow rate of argon is 300NL / min;
[0043] (3) Power transmission and slag operation, the secondary voltage of the transformer is maintained at 278V, and the flow rate of argon gas is 130NL / min;
[0044] (4) After the slag has been completely melted and thoroughly deoxidized, the order of adding the deoxidizer is to add silicon carbide first and then calcium carbide, the amount of silicon carbide added per ton of steel is 0.4kg, the amount of calcium carbide added per ...
Embodiment 3
[0048] For A36B steel, process steps:
[0049] (1) Slag washing is carried out during the tapping process of the converter, and the amount of lime added per ton of steel is 2.5kg;
[0050] (2) Move the ladle to the refining treatment position, the refining start temperature is 1520°C, the amount of lime added per ton of steel is 5.0kg, the amount of fluorite added per ton of steel is 1.2kg, and the feeding time is 3min. The flow rate is 240NL / min;
[0051] (3) Power transmission and slag operation, the secondary voltage of the transformer is maintained at 313V, and the flow rate of argon gas is 140NL / min;
[0052] (4) Deoxidize after the slag has been fully melted and thoroughly deoxidized. The order of adding the deoxidizer is to add silicon carbide first and then calcium carbide. The amount of silicon carbide added per ton of steel is 0.25 kg, and the amount of calcium carbide added per ton of steel is 0.5 kg. The slag sample is yellow and white slag; The accumulated amoun...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com