A sign and traffic technology, applied in the field of traffic signs, can solve the problems that need to be improved and the surface finish is not ideal, and achieve the effect of excellent rust prevention and good surface finish.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Example Embodiment
[0024] Example 1
[0025] A traffic sign includes a metal plate main body, the metal plate main body is passivated, and the passivation includes the following steps:
[0026] 1) Put 1 to 2 parts by weight of phosphoric acid ester, 4.1 parts by weight of phosphotungstic acid, 5.1 parts by weight of fluorozirconic acid, 0.9 parts by weight of sodium benzoate, and 1.3 parts by weight of hydrogen peroxide into 30 parts by weight of deionized water, and stir well ;
[0027] 2) Then add 3.6 parts by weight of hexyldecanol, 1.6 parts by weight of alkyltrimethylammonium methanesulfate, 1.8 parts by weight of 1-hydroxybenzotriazole, 2.5 parts by weight of alkylphenol polyoxyethylene ether, 4.1 parts by weight of two Propylene glycol, continue to stir, until fully mixed and uniform, to prepare passivation treatment liquid;
[0028] 3) Put the metal plate main body into the passivation treatment liquid for passivation treatment, the treatment temperature is 37° C., the treatment time is 43 seco...
Example Embodiment
[0029] Example 2
[0030] A traffic sign includes a metal plate main body, the metal plate main body is passivated, and the passivation includes the following steps:
[0031] 1) Put 1 part by weight of phosphoric acid ester, 4.1 parts by weight of phosphotungstic heteropoly acid, 5.1 parts by weight of fluozirconic acid, 0.9 parts by weight of sodium benzoate, and 1.3 parts by weight of hydrogen peroxide into 30 parts by weight of deionized water in sequence, and stir evenly;
[0032] 2) Then add 3.6 parts by weight of hexyldecanol, 1.6 parts by weight of alkyltrimethylammonium methanesulfate, 1.8 parts by weight of 1-hydroxybenzotriazole, 2.5 parts by weight of alkylphenol polyoxyethylene ether, 4.1 parts by weight of two Propylene glycol, continue to stir, until fully mixed and uniform, to prepare passivation treatment liquid;
[0033] 3) Put the metal plate main body into the passivation treatment liquid for passivation treatment, the treatment temperature is 37° C., the treatment ...
Example Embodiment
[0034] Example 3
[0035] A traffic sign includes a metal plate main body, the metal plate main body is passivated, and the passivation includes the following steps:
[0036] 1) Put 2 parts by weight of phosphate ester, 4.1 parts by weight of phosphotungstic heteropoly acid, 5.1 parts by weight of fluozirconic acid, 0.9 parts by weight of sodium benzoate, and 1.3 parts by weight of hydrogen peroxide into 30 parts by weight of deionized water, and stir evenly;
[0037] 2) Then add 3.6 parts by weight of hexyldecanol, 1.6 parts by weight of alkyltrimethylammonium methanesulfate, 1.8 parts by weight of 1-hydroxybenzotriazole, 2.5 parts by weight of alkylphenol polyoxyethylene ether, 4.1 parts by weight of two Propylene glycol, continue to stir, until fully mixed and uniform, to prepare passivation treatment liquid;
[0038] 3) Put the metal plate main body into the passivation treatment liquid for passivation treatment, the treatment temperature is 37° C., the treatment time is 43 second...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap