Production method of imitation hollowed-out artwork
A production method and decoration technology, which is applied in the field of production of imitation hollow carving decorations, can solve the problems of complex production process, difficult to widely use, high cost, etc., and achieve the effect of simple process, not easy to pollute and deform, and low price
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0010] Making imitation hollow-out carved decorative surface of heating cover
[0011] 1. The mold of the carved product
[0012] Use wood or wax boards with the required thickness and size. After the surface treatment is smooth, draw the designed patterns and carve to complete a hollowed-out decorative surface of the heating hood. After multiple modifications, polish it as a mold.
[0013] 2. Make molds by using moulds.
[0014] ① Fix the carved mold on a wooden board that is 15-25mm larger than its surroundings, and deal with the gaps between them. Fix the wooden strips around the board that are 5-10mm higher than the highest point of the mold as a baffle , deal with the gap, put it on the platform and prepare for molding.
[0015] ②Measure the volume of the mould, inject the required silica gel according to the required capacity, release the mold after curing, and trim the burrs to complete the silica gel mold.
[0016] ③ Attach the prepared silicone mold to a plate of t...
Embodiment 2
[0025] Making imitation hollow carved screen surface
[0026] 1. The mold of the carved product
[0027] A hollow carved screen surface (or a screen surface unit) is completed as a mold according to the method of Embodiment 1.
[0028] 2. Make molds by using moulds.
[0029] Method is the same as embodiment one.
[0030] 3. Prepare pouring materials for imitation hollow carving products
[0031] Take 5Kg of low-shrinkage unsaturated polyester resin, 0.05Kg of methyl ethyl ketone peroxide curing agent, 0.05Kg of cobalt isooctanoate accelerator, and 1.5Kg of light calcium carbonate filler, and mix them uniformly to make casting materials.
[0032] 4. Product molding
[0033] Method is the same as embodiment one.
[0034] 5. Finished product processing
[0035] Method is the same as embodiment one.
Embodiment 3
[0037] Making imitation hollow carved windows
[0038] 1. The mold of the carved product
[0039] Complete a hollow carved window as a mold by the method of Embodiment 1.
[0040] 2. Make molds by using moulds.
[0041] Method is the same as embodiment one.
[0042] 3. Prepare pouring materials for imitation hollow carving products
[0043] Take 2Kg of low-shrinkage unsaturated polyester resin, 0.02Kg of methyl ethyl ketone peroxide curing agent, 0.02Kg of cobalt isooctanoate accelerator, and 0.6Kg of light calcium carbonate and mix them evenly to prepare casting materials.
[0044] 4. Product molding
[0045] Take half of the raw material and pour it into the required casting part in the silicone mold, then place glass fiber on the poured raw material (mainly placed in the weaker structure), and then perform the second pouring to fill the raw material to the upper plane of the silicone mold . After curing, turn it over together with the bottom plate, remove the bottom p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com