[0017] Use 60Nm wet-spun hemp yarns as warp and weft yarns to produce 60Nm×60Nm×68×68×63″ wet-spun hemp flat cloth. The manufacturing method: 60Nm warp and weft yarns are all passed through automatic winding machines. The process is: short thick knots: 220% 3.0 cm; long slub: 90% 40cm; detail: -70% 59cm, relative humidity: 75%, temperature: 25℃.
[0018] The steam heat and humidity twist setting method is adopted, and the process requires a steam pressure of 8 MPa and a time of 28 minutes.
[0019] Batch warping machine is used for warping, pneumatic pressure is applied, and the warping tension is divided into four zones and three layers. Single warp yarn tension is 75cN, side warp yarn tension increases 20%, speed: 200 m / min.
[0020] The sizing is carried out on a Ben-procome sizing machine, using wet split stranding. Sizing formula: modified starch: 60%, polymethyl acrylate: 30%, polyvinyl alcohol: 10%, high sizing rate, count yarn: 10-12%, moisture regain: 7.5%, elongati...
example 2
[0024] Use 24Nm wet-spun hemp yarns as warp and weft yarns to produce 24Nm×24Nm×54×54×63″ wet-spun hemp plain cloth: the 24Nm warp and weft yarns are all passed through the automatic winder. The process is: short thick knots: 220% 3.0 cm; long thick quarter: 90% 40cm; detail: -70% 59cm, relative humidity: 70%, temperature: 22℃.
[0025] Adopt steam heat wet twist fixing method, process requires steam pressure 16MPa, time 15 minutes (or steam pressure 0.12MPa, time 30 minutes).
[0026] Batch warping machine is used for warping, pneumatic pressure is applied, and the warping tension is divided into three zones and three layers. Single warp yarn tension is 65cN, side warp yarn tension increases by 25%, speed: 300 m / min.
[0027] The sizing is carried out on a Ben-procome sizing machine, using wet split stranding. Sizing formula: modified starch: 80%, polymethyl acrylate: 20%, polyvinyl alcohol: 0%, sizing rate medium-count yarn is 7.1-9.9%, moisture regain: 6%, elongation: 0.5...
example 3
[0031] Use 7Nm wet-spun hemp yarn as warp and weft yarn to produce 7Nm×7Nm×41×30×63″ wet-spun hemp flat cloth. The manufacturing method: 7Nm yarns are all passed through ordinary winding machines, equipped with water mist air twister and electronic yarn clearing device, metal groove tube, and length fixer. The process is: short thick place: 220% 3.0cm; long thick place: 90% 40cm; detail: -70% 59cm, made into non-joint yarn, strand twist: 10 twists / inches, relative humidity: 73%, temperature: 26°C.
[0032] The yarn is placed in a humidification chamber with a temperature of 36° C. and a relative humidity of 78% (or a temperature of 32° C. and a relative humidity of 75%) for 24 hours for yarn setting.
[0033] Batch warping machine is used for warping, pneumatic pressure is applied, and the warping tension is divided into three zones and three layers. Single warp yarn tension is 95cN, side warp yarn tension increases by 22%, warping speed: 180 m / min. Inverting axis speed: 10...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap