A moisture-proof wall coating
A coating and raw material technology, applied in the direction of rubber derivative coatings, coatings, etc., can solve the problems of low bonding strength, non-friction resistance, water resistance and poor low temperature stability, and achieve good wear resistance and smooth and beautiful appearance Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A kind of moisture-proof wall surface paint, its raw material ratio is as follows in parts by weight: 100 parts of polyvinyl alcohol; 40 parts of modified bentonite; 25 parts of absolute ethanol; 30 parts of xylene; 65 parts of ionized water; 60 parts of chlorinated rubber; 10 parts of light calcium carbonate; 45 parts of talcum powder; 65 parts of ammonia water; 10 parts of titanium dioxide; 4 parts of dibutyl phthalate; 5 parts of zinc phosphate; 35 parts of water glass 40 parts of epoxidized soybean oil.
[0016] After dissolving epoxidized soybean oil in deionized water, add light calcium carbonate and isinglass, use a ball mill to mill for 30 minutes, add ammonia water, polyvinyl alcohol, modified bentonite, absolute ethanol, xylene and paraffin, mill for 30 minutes, add Chlorinated rubber and remaining raw materials were ball-milled for 1 hour and then filtered with gauze to obtain the finished product.
[0017] The product has good wear resistance, 0.006g / cm2 fo...
Embodiment 2
[0019] A kind of moisture-proof wall surface paint, its raw material ratio is as follows by weight: 100 parts of polyvinyl alcohol; 50 parts of modified bentonite; 35 parts of dehydrated alcohol; 40 parts of xylene; 30 parts of isinglass; 85 parts of ionized water; 80 parts of chlorinated rubber; 20 parts of light calcium carbonate; 55 parts of talcum powder; 75 parts of ammonia water; 20 parts of titanium dioxide; 10 parts of dibutyl phthalate; 15 parts of zinc phosphate; 45 parts of water glass ; 50 parts of epoxidized soybean oil.
[0020] After dissolving epoxidized soybean oil in deionized water, add light calcium carbonate and isinglass, use a ball mill to mill for 30 minutes, add ammonia water, polyvinyl alcohol, modified bentonite, absolute ethanol, xylene and paraffin, mill for 30 minutes, add Chlorinated rubber and remaining raw materials were ball-milled for 1 hour and then filtered with gauze to obtain the finished product.
[0021] The product has good wear resis...
Embodiment 3
[0023] A kind of moisture-proof wall surface paint, its raw material ratio is as follows by weight: 100 parts of polyvinyl alcohol; 45 parts of modified bentonite; 30 parts of absolute ethanol; 35 parts of xylene; 25 parts of isinglass; 75 parts of ionized water; 70 parts of chlorinated rubber; 15 parts of light calcium carbonate; 50 parts of talcum powder; 70 parts of ammonia water; 15 parts of titanium dioxide; 7 parts of dibutyl phthalate; 10 parts of zinc phosphate; 40 parts of water glass ; 45 parts of epoxidized soybean oil.
[0024] After dissolving epoxidized soybean oil in deionized water, add light calcium carbonate and isinglass, use a ball mill to mill for 30 minutes, add ammonia water, polyvinyl alcohol, modified bentonite, absolute ethanol, xylene and paraffin, mill for 30 minutes, add Chlorinated rubber and remaining raw materials were ball-milled for 1 hour and then filtered with gauze to obtain the finished product.
[0025] The product has good wear resistan...
PUM
Login to View More Abstract