Embodiment 1
[0015] (1) Weigh 1Kg of gravel with a crushing value of 9.5-13.2, 2Kg of crushed stone with a crushing value of 4.75-9.5, and 1Kg of stone chips, and mix them into aggregates;
[0016] (2) Weigh 10% powder anti-stripping agent, 10% mineral powder, 20% polymer rubber powder and 50% sulphoaluminate cement to make a concentrated curing agent, and weigh the yellow concentrated curing Add 60g (1.5%) of the curing agent, put the above aggregate and curing agent into the mixing pot and stir for 30s;
[0017] (3) Weigh 80g (2%) of water, add it into the stirring pot and continue stirring for 30s;
[0018] (4) Weigh 380g (9.5%) of asphalt liquid at room temperature, add it into the mixing pot and continue to stir for 60s, the mixed material can be kneaded without loosening and stirred evenly;
[0019] (5) Make 3 standard Marshall test pieces from the mixed material, weigh 1.3Kg of the mixed material for each test piece, and compact 50 times on both sides;
[0020] (6) Mix one pot aga...
Embodiment 2
[0024] (1) Weigh 1.1Kg of gravel with a crushing value of 9.5-13.2, 2.2Kg of crushed stone with a crushing value of 4.75-9.5, and 1Kg of stone chips, and mix them into aggregate;
[0025] (2) Weigh 12% powder anti-stripping agent, 15% mineral powder, 25% polymer rubber powder and 65% sulphoaluminate cement to make a concentrated curing agent, and weigh the yellow concentrated curing 75g (1.5%) of the agent, put the above aggregate and curing agent into the mixing pot and stir for 30s;
[0026] (3) Weigh 90g (2%) of water, add it into the stirring pot and continue stirring for 30s;
[0027] (4) Weigh 420g (9.5%) of asphalt liquid at room temperature, add it into the mixing pot and continue to stir for 60s, and the mixed material can be kneaded without loosening and stirred evenly;
[0028] (5) Make 3 standard Marshall test pieces from the mixed material, weigh 1.3Kg of the mixed material for each test piece, and compact 50 times on both sides;
[0029] (6) Mix one pot again a...
Embodiment 3
[0033] (1) Weigh 1.25Kg of crushed stones with a crushing value of 9.5-13.2, 2.5Kg of crushed stones with a crushing value of 4.75-9.5, and 1.25Kg of stone chips, and mix them into aggregates;
[0034] (2) Weigh 15% powder anti-stripping agent, 20% mineral powder, 30% polymer rubber powder and 70% sulphoaluminate cement to make a concentrated curing agent, and weigh the yellow curing agent 90g (1.5%), put the above aggregate and curing agent into the stirring pot and stir for 30s;
[0035] (3) Weigh 100g (2%) of water, add it into the stirring pot and continue stirring for 30s;
[0036] (4) Weigh 475g (9.5%) of normal-temperature asphalt liquid, weigh 10g of rock asphalt solution and add it to the normal-temperature asphalt liquid and stir for 2 minutes, then add them into the stirring pot and continue stirring for 60 seconds, and the resulting mixture can be kneaded without loosening;
[0037] (5) Mix 4-6 pots of mixture in this way (too much mixture at one time is not easy ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com