A mink skin and tanning technology, which is applied in leather manufacturing, leather degreasing, leather drying, etc., can solve the problems of wasting water resources, large water consumption, and increasing costs, and achieve the effects of reducing consumption, reducing content, and reducing costs
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2016-09-28
Abstract
Description
Technical field:
[0001] The invention relates to the field of fur production, in particular to a process for tanning mink fur. Background technique:
[0002] In the prior art, the mink skin tanning process is simple, and the water in the workshop is treated in a straight line, which cannot effectively collect valuable water for reuse, and the water consumption is large, which not only increases the cost but also wastes water resources. Invention content:
[0003] The technical problem to be solved by the invention is to provide an energy-saving and environment-friendly mink skin tanning process.
[0004] Technical solution of the present invention is to provide a kind of mink skin tanning process, it comprises the following steps:
[0005] The first step is to wash the skin, soak the skin in the skin washing water, control the temperature at 24-26°C, add bactericide, degreasing agent, grease dispersant, after 2 hours, dry the skin, and directly discharge the water into th...
Examples
Embodiment
[0027] A kind of mink fur tanning process, it comprises the following steps:
[0028] The first step is to wash the skin, soak the skin in the skin washing water, control the temperature at 24-26°C, add bactericide, degreasing agent, grease dispersant, after 2 hours, dry the skin, and directly discharge the water into the sewage treatment tank ;
[0029] The second step is to roll the wood chaff to remove the grease, put the skin into the wooden drum, add the fine wood chaff, add the degreasing agent, turn for 1.5-2 hours, and leave the drum;
[0030] The third step is to use a round knife to cut off the excess fat on the head, backline and tail with a disc shaving machine;
[0031] The fourth step is to pull oil, use a wire oil machine to pull the whole body, so that the whole body is clean and free of oil lumps;
[0032] The fifth step is degreasing. Soak the skin in water at 36-38°C, add salt, bactericide, degreasing agent, penetrant, and grease dispersant for 2 hours, re...