preparation example Construction
[0027] The invention provides a method for preparing a negative electrode with a protective layer, comprising the following steps:
[0028] mixing the alkali metal salt and the anion acceptor compound to obtain an electrolyte solution;
[0029] Coating the electrolyte solution on the working surface of the negative electrode of the battery and drying it to obtain a negative electrode with a protective layer;
[0030] The anion acceptor compound comprises (C 6 h 3 F)O 2 B(C 6 h 3 f 2 ), (C 6 f 4 )O 2 B(C 6 f 5 ), TPFPB, [(CF 3 )CHO] 3 B.(C 6 f 5 O) 3 B. One or more of fluoroethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate and TMSB.
[0031] In the present invention, unless otherwise specified, all preparation materials are commercially available products well known to those skilled in the art.
[0032] The invention mixes alkali metal salt and anion acceptor compound to obtain electrolytic solution. In the present invention, th...
Embodiment 1
[0053] 2g LiF and 50mL tris(trimethylsilane) borate were mixed to obtain an electrolyte solution;
[0054] 0.1mL of the electrolyte solution was added dropwise on the working surface of the metal lithium sheet, and dried in a glove box to obtain a negative electrode with a protective layer;
[0055] With the aluminum flake as the positive electrode current collector, the ternary material NCM811 as the positive electrode active material, and the negative electrode with the protective layer as the negative electrode, the positive electrode, the diaphragm, and the electrolyte (concentration is 1.5mol / L; the solvent is the volume ratio of 1:1 mixture of EC and DMC; solute is LiPF 6 ) and a negative electrode installation with a protective layer to prepare a lithium metal battery;
[0056] The protective layer in the negative electrode with protective layer is carried out SEM test, test result is as follows figure 1 shown by figure 1 It can be seen that the surface of Li metal i...
Embodiment 2
[0058] Mix 2g NaF and 50mL fluoroethylene carbonate to obtain an electrolyte solution;
[0059] After adding 0.1 mL of the electrolyte solution dropwise on the working surface of the metal sodium sheet, dry it in a glove box to obtain a negative electrode with a protective layer;
[0060] With the aluminum flake as the positive electrode current collector, the ternary material NCM811 as the positive electrode active material, and the negative electrode with the protective layer as the negative electrode, the positive electrode, the diaphragm, and the electrolyte (concentration is 1.5mol / L; the solvent is the volume ratio of 1:1 mixture of EC and DMC; solute is NaPF 6 ) and a negative electrode with a protective layer are installed to obtain a sodium metal battery.