Looking for breakthrough ideas for innovation challenges? Try Patsnap Eureka!

Method for obtaining high-pearlite high-tenacity nodular cast iron crankshaft

A technology of nodular cast iron and pearlite, which is applied in the field of heat treatment, can solve the problems of insufficient plastic reserve, large consumption of normalizing liquid, and inconvenient machining, and achieve good machining performance, save loss costs, and save costs.

Inactive Publication Date: 2010-12-22
荆州环宇汽车零部件有限公司
View PDF3 Cites 4 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The pearlite content of the cast iron is greater than (equal to) 95%, cementite ≤ 5%, and the tensile strength can reach 700-850N / mm 2 , hardness 280-350HB, elongation 3%-5%, its disadvantages are: 1 low tensile strength, only 700N / mm 2 , cannot be used on crankshaft products above QT800-2. 2. The hardness is as high as 350HB and the machinability is poor, which brings inconvenience to machining. 3. The lower limit of elongation is 3%, the upper limit is 5%, and the plastic reserve is insufficient.
[0004] The second is the "Trial Production of Cast Pearlitic Ductile Iron 276Q Crankshaft" published by Chen Lianta of Liuzhou Machinery Factory in Guangxi, which proposed the use of rare earth magnesium nodularizers to produce as-cast pearlitic ductile iron by the flushing method. The pearlite content up to 90-95%, the shortcoming of this technology is that the pearlite content can not reach more than 95% stably
[0005] The third is the method of using normalizing liquid to obtain pearlite ≥ 95% proposed by Industrial Furnace Information Network in "Application of Ideal Normalizing Liquid": heating the as-cast crankshaft to 940°C for 2 hours and then adding to the normalizing liquid Medium cooling, then heating to 550°C for 1.5 hours, tempering and water cooling, so as to obtain a pearlite ≥ 95% metallographic structure and a tensile strength of 855N / mm 2 , the elongation rate is 3.6%, and the mechanical properties of hardness HB are 277. The defects of this technology are: 1 normalizing liquid is 20,000 yuan / ton, the price is expensive, and the normalizing liquid consumes a lot during normalizing cooling, and the normalizing cost is relatively high. High, 2. The above properties can only be obtained by tempering at 550°C for 2 hours, and the production cost is higher. 3. The elongation rate is 3.6% and the plastic reserve is insufficient

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for obtaining high-pearlite high-tenacity nodular cast iron crankshaft
  • Method for obtaining high-pearlite high-tenacity nodular cast iron crankshaft
  • Method for obtaining high-pearlite high-tenacity nodular cast iron crankshaft

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0029] CA4102 crankshaft material requirements: QT800-2, hardness requirements: HB 260-300.

[0030] 1. Melting furnace: 1 ton electric furnace, molten iron weight 1045Kg, plus nodulizer rare earth magnesium 11Kg

[0031] Chemical composition of materials before spheroidization:

[0032]

[0033] Chemical composition of materials after spheroidization:

[0034]

[0035] 2. Pouring: The temperature of molten iron coming out of the furnace: 1493°C;

[0036] Casting pouring temperature: 1428°C;

[0037] 3. Unpacking and demoulding: the interval between the pouring of crankshaft castings and the start of unpacking is 13 minutes;

[0038] When unpacking, the casting surface temperature is 899°C; the ambient temperature is 34°C;

[0039] 4. The surface temperature of the crankshaft casting is 849°C when the blowing cooling starts; cool the crankshaft casting to the ambient temperature by blowing blowing;

[0040] 5. Cool the crankshaft casting until the ambient temperatur...

Embodiment 2

[0051] YTR4105 crankshaft material requirements: QT800-2, hardness requirements: HB 240-320;

[0052] 1. Melting furnace: 1 ton electric furnace, molten iron weight 1070Kg, plus nodulizer rare earth magnesium 11Kg

[0053] Chemical composition of materials before spheroidization:

[0054]

[0055] After spheroidizing the chemical composition of the material:

[0056]

[0057] 2. Pouring: The temperature of molten iron coming out of the furnace: 1493°C;

[0058] Casting pouring temperature: 1392°C;

[0059] 3. Unpacking and demoulding: the interval between casting pouring and unpacking is 12 minutes and 58 seconds;

[0060] The surface temperature of the crankshaft casting is 891°C when the box is opened; the ambient temperature is 34°C;

[0061] 4. The surface temperature of the crankshaft casting is 860°C when the air blowing is started to cool down; the crankshaft casting is cooled to the ambient temperature by air blowing;

[0062] 5. Cool the crankshaft castings...

Embodiment 3

[0073] YTR4105 crankshaft material requirements: QT800-2, hardness requirements: HB 240-320;

[0074]1. Melting furnace: 1.5 tons of electric furnace, molten iron weight 1485Kg, plus nodulizer rare earth magnesium 15Kg Material chemical composition:

[0075] Chemical composition of materials before spheroidization:

[0076]

[0077] Chemical composition of materials after spheroidization:

[0078]

[0079] Hot metal out of furnace temperature: 1492°C;

[0080] 2. Pouring: Casting pouring temperature: 1389°C;

[0081] The interval between the end of casting pouring and the start of unpacking is 12 minutes and 48 seconds;

[0082] 3. Unpacking and demoulding: when unpacking, the surface temperature of the crankshaft casting is 887°C; the ambient temperature is 34°C;

[0083] 4. The surface temperature of the crankshaft casting is 857°C when the air blowing is started to cool down; cool the crankshaft casting to the ambient temperature by air blowing;

[0084] 5. Cool ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
hardnessaaaaaaaaaa
elongationaaaaaaaaaa
elongationaaaaaaaaaa
Login to View More

Abstract

The invention relates to a method for obtaining a high-pearlite high-tenacity nodular cast iron crankshaft by improving the pearlite content of nodular cast iron and improving the mechanical properties. For a nodular cast iron crankshaft casting containing less than 0.82% of Mn, after treatment of the casting by a double normalizing process of residual heat normalizing and general normalizing, the pearlite content of the nodular cast iron crankshaft casting is greater than or equal to 95%, the elongation is greater than or equal to 5%, and HB is greater than or equal to 260. The invention dispenses with the cost of adding Cu and the cost of normalizing liquid and consumption thereof, and enables the pearlite content of the nodular cast iron crankshaft casting to be greater than or equal to 95% and the nodular cast iron crankshaft casting to have favorable mechanical properties.

Description

technical field [0001] The present invention relates to heat treatment, in particular to a method for high pearlite content and improved mechanical properties of nodular cast iron. Background technique [0002] The role of pearlite in ductile iron is very obvious. It can increase the tensile strength and hardness of ductile iron and improve its mechanical properties. At present, there are three ways to increase the content and methods of pearlite in ductile iron: [0003] The first one is "Research on new cast high-strength pearlite ductile iron" published by Zhu Xianyong and Liu Yaohui from the School of Materials Science and Engineering of Jilin University in "Journal of Materials Heat Treatment" 2007 02 and in February 2007 in agricultural machinery The "Microstructure and Properties of As-Cast Pearlite Ductile Iron" published in the second issue of Volume 38 of the Journal of the Chinese Academy of Sciences proposed the same method for obtaining a pearlite content great...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C21D9/30C21D5/00
Inventor 王锦焱徐阳王宝文蒋在春
Owner 荆州环宇汽车零部件有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products