Wide High Density Fabric Rolls
A technology of fabric rolls and fabrics, applied in the direction of fabrics, textiles, winding strips, etc., can solve the problems of unusable fabrics, etc., and achieve the effect of excellent quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0077] Fibers having a strength of 8 cN / dtex obtained by melt-spinning and thermally stretching polyhexamethylene adipamide resin were used as the warp and weft of the fabric. The fiber has a fineness of 470 dtex, 136 filaments, a boiling water shrinkage of 7.0%, and an interlacing number of 10 / m by water immersion. The warp yarns were warped without twisting and without glue, and warp yarn bundles with 4428 warp yarns were produced. The number of reinforcing yarns in the selvage portion was set to 4 on one side and 8 on both sides, the fineness of the reinforcing yarns were all set to 22 dtex, and the fineness of the leno yarn was also set to 22 dtex. In addition, the number of warp yarns entered into the reed (the number of warp yarns per one reed dent) was set to 1 / reed dent.
[0078] A water-jet loom was used as a loom, and the warp tension was set at 0.32 cN / dtex, and weaving was carried out using the same yarn as the warp for the weft at a loom rotation speed of 700 rpm...
Embodiment 2
[0083] The warp tension at the time of weaving was set to 0.21 cN / dtex, and the winding tension to the paper tube in the subsequent process was set to 0.7 N / cm, and it was implemented in the same manner as in Example 1.
[0084] The evaluation results of the obtained fabric rolls are shown in Table 1 below. The yarn tail length of the fabric is 4mm, the roll hardness of the fabric is 78° at the center, and the difference between the roll hardness at the end is 5°, and the unevenness of the fabric roll surface is 0.4%. In addition, the state of the fabric when the fabric roll is unwound , The quality of the fabric selvedge has also become a good result.
Embodiment 3
[0086] The fineness of the warp and weft yarns used is set to 700dtex, the monofilament is set to 105, and a warp yarn bundle with 3600 warp yarns is made, and the warp yarn tension during weaving is set to 0.38cN / dtext. Implementation under the same conditions as in Example 1.
[0087] The evaluation results of the obtained fabric rolls are shown in Table 1 below. The yarn tail length of the fabric is 5 mm, the roll hardness of the fabric is 82° at the center, and the difference between the roll hardness at the end is 4°, and the unevenness of the fabric roll surface is 0.7%. In addition, the state of the fabric when the fabric roll is unwound , The quality of the fabric selvedge has also become a good result.
PUM
| Property | Measurement | Unit |
|---|---|---|
| width | aaaaa | aaaaa |
| length | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |