A flaky silver powder and anti-oxidation technology, which is applied in the field of flaky silver powder and its preparation, can solve the problems of affecting anti-counterfeiting performance, flaky silver powder is easy to oxidize, etc., and achieve the effect of improving anti-oxidation performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0051] The content of the antioxidant flake silver powder is specifically:
[0052] 6-8 micron flake silver powder 10 kg
[0053] High purity water 10 liters
[0054] Silver protectant 200g
[0055] The preparation method is as follows:
[0056] a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat it to 80°C;
[0057] b. Weigh 10 kilograms of flake silver powder and 200 grams of silver protective agent (Shenzhen Ezhen Technology Co., Ltd. EZ-AGII water-soluble silver protective agent can be selected), and place them in the container;
[0058] c. Stir fully after soaking for 1 hour;
[0059] d. Pour the aqueous solution of the flake silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0060] e. Obtain anti-oxidation flake silver powder after drying.
Embodiment 2
[0061] Example 2: The content of the antioxidant flake silver powder is specifically:
[0062] 6-8 micron flake silver powder 10 kg
[0063] High purity water 10 liters
[0064] Silver protector 300g
[0065] The preparation method is as follows:
[0066] a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat it to 80°C;
[0067] b. Weigh 10 kilograms of flake silver powder and 300 grams of silver protective agent (Shenzhen Ezhen Technology Co., Ltd. EZ-AGII water-soluble silver protective agent can be used), and place them in the container;
[0068] c. Stir fully after soaking for 1 hour;
[0069] d. Pour the aqueous solution of the flake silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0070] e. Obtain anti-oxidation flake silver powder after drying.
Embodiment 3
[0072] The content of the antioxidant flake silver powder is specifically:
[0073] 6-8 micron flake silver powder 10 kg
[0074] High purity water 10 liters
[0075] Silver protectant 400g
[0076] The preparation method is as follows:
[0077] a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat it to 80°C;
[0078] b. Weigh 10 kilograms of flake silver powder and 400 grams of silver protective agent (Shenzhen Ezhen Technology Co., Ltd. EZ-AGII water-soluble silver protective agent can be used), and place them in the container;
[0079] c. Stir fully after soaking for 1 hour;
[0080] d. Pour the aqueous solution of the flake silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0081] e. Obtain anti-oxidation flake silver powder after drying.