A kind of robot spraying car surfacer paint
A primer and robot technology, used in coatings, conductive coatings, polyurea/polyurethane coatings, etc., can solve the problems of high baking temperature, high price, high energy consumption, etc., to improve settling resistance, improve Anti-prickly heat performance, good effect of long-distance pipeline transportation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0021] In this embodiment, the robot sprays the automobile surfacer, which is composed of main paint, curing agent and thinner, and the main paint is composed of the following components in parts by weight: 26 parts of acrylic resin 802, 8 parts of polyester resin 803, titanium dioxide 25 parts, 12 parts of superfine talc powder, 0.5 parts of fumed silica, 0.5 parts of BYK110, 8 parts of zinc phosphate, 2 parts of ES80, 20 parts of mixed solvents of lipids and benzene, including: 12 parts of butyl acetate, xylene 5 parts, 3 parts of PMA; 55 parts of N75 in the curing agent, 45 parts of butyl acetate; a total of 100 parts of diluent, including: 20 parts of butyl acetate, 40 parts of xylene, 30 parts of PMA, and 10 parts of DBE.
[0022] The preparation method of robot spraying automobile surfacer in the present embodiment comprises the following steps:
[0023] (1) Main paint: Accurately take each component according to the parts by weight, add 26 parts of acrylic resin 802, 80...
Embodiment 2
[0028] In this embodiment, the robot sprays the automobile surfacer, which is composed of main paint, curing agent and thinner, and the main paint is composed of the following components in parts by weight: 20 parts of acrylic resin 802, 8 parts of polyester resin 803, titanium dioxide 25 parts, 18 parts of superfine talc powder, 0.5 parts of fumed silica, 0.5 parts of BYK110, 8 parts of zinc phosphate, 2 parts of ES80, 20 parts of mixed solvents of lipids and benzene, including: 12 parts of butyl acetate, xylene 5 parts, 3 parts of PMA; 55 parts of N75 in the curing agent, 45 parts of butyl acetate; a total of 100 parts of diluent, including: 20 parts of butyl acetate, 40 parts of xylene, 30 parts of PMA, and 10 parts of DBE.
[0029] When used, the volume ratio of main paint to curing agent and thinner is 40:10:15.
[0030] In this embodiment, the preparation method of robot spraying automobile surfacer is the same as that of Embodiment 1.
Embodiment 3
[0032] In this embodiment, the robot sprays the automobile surfacer, which is composed of main paint, curing agent and thinner, and the main paint is composed of the following components in parts by weight: 26 parts of acrylic resin 802, 8 parts of polyester resin 803, titanium dioxide 25 parts, 12 parts of superfine talcum powder, 0.5 parts of fumed silica, .5 parts of BYK1100, 8 parts of zinc phosphate, 20 parts of mixed solvents of lipids and benzene, including: 12 parts of butyl acetate, 5 parts of xylene, 3 parts of PMA; 55 parts of N75 in curing agent, 45 parts of butyl acetate; 100 parts of diluent in total, including: 20 parts of butyl acetate, 40 parts of xylene, 30 parts of PMA, and 10 parts of DBE.
[0033] When used, the volume ratio of main paint to curing agent and thinner is 40:10:15.
[0034] In this embodiment, the preparation method of robot spraying automobile surfacer is the same as that of Embodiment 1.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 