Thermoplastic coating suitable for tinplate and aluminum foil heat sealing and preparation method thereof
A thermoplastic and tinplate technology, applied in the direction of polyester coatings, coatings, etc., can solve the problems of poor peeling appearance, etc., and achieve the effect of simple production process, low production process requirements, and easy access to raw materials
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] This embodiment relates to a thermoplastic coating suitable for heat sealing tinplate and aluminum foil, and its preparation specifically includes the following steps:
[0035] (1) Prepare raw materials according to the following components and contents (parts by weight)
[0036] Component
parts by weight
polyester resin
1
Butyl Methacrylate Segmented Acrylic Resin
5
Ternary vinyl resin
14
Mercaptan Organotin Heat Stabilizer
0.005
28
20
20
Propylene Glycol Methyl Ether
12
Anti-abrasion agent Polyethylene micronized wax
0.08
[0037] (2) Add ethyl acetate, n-propyl acetate, butanone, propylene glycol methyl ether, and heat stabilizer into the reaction kettle, turn on the mixer to a medium speed of 750-800 rpm, and keep the temperature at 50°C;
[0038] (3) Add acrylic resin and vinyl chloride resin into the reaction kettle, s...
Embodiment 2
[0043] This embodiment relates to a thermoplastic coating suitable for heat sealing tinplate and aluminum foil, and its preparation specifically includes the following steps:
[0044] (1) Prepare raw materials according to the (weight parts) raw materials of the following components and contents:
[0045] Component
parts by weight
4
Butyl Methacrylate Segmented Acrylic Resin
6
Ternary vinyl resin
10
Mercaptan Organotin Heat Stabilizer
0.005
28
20
20
Propylene Glycol Methyl Ether
12
Anti-abrasion agent Polyethylene micronized wax
0.08
[0046] (2) Add ethyl acetate, n-propyl acetate, butanone, propylene glycol methyl ether, and heat stabilizer into the reaction kettle, turn on the mixer to a medium speed of 700-750 rpm, and keep the temperature at 50°C;
[0047] (3) Add acrylic resin and vinyl chloride resin into the...
Embodiment 3
[0052] This embodiment relates to a thermoplastic coating suitable for heat sealing tinplate and aluminum foil, and its preparation specifically includes the following steps:
[0053] (1) Prepare raw materials according to the (weight parts) raw materials of the following components and contents:
[0054] Component
parts by weight
6
Butyl Methacrylate Segmented Acrylic Resin
6
Ternary vinyl resin
8
Mercaptan Organotin Heat Stabilizer
0.01
ethyl acetate
28
20
butanone
20
Propylene Glycol Methyl Ether
12
Anti-abrasion agent Polyethylene micronized wax
0.09
[0055] (2) Add ethyl acetate, n-propyl acetate, butanone, propylene glycol methyl ether, and heat stabilizer into the reaction kettle, turn on the mixer to a medium speed of 720-750 rpm, and keep the temperature at 40°C;
[0056] (3) Add acrylic resin and vinyl chloride resin into the r...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 