Method for digitally and controllably printing ITO (Indium Tin Oxide) nanowires

A nanowire and digital technology, applied in the direction of nanotechnology, nanotechnology, nanotechnology for materials and surface science, etc., can solve the problems of unfriendly environment, low yield, high cost of nanowires, etc., and achieve easy operation and high production efficiency The effect of high efficiency and excellent light transmission performance

Pending Publication Date: 2022-07-12
NANKAI UNIV
View PDF5 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The preparation of ITO nanowires by the method of the present invention not only has the advantages of low cost, high yield, energy saving and environmental protection, simple process, easy operation, suitable for large-scale preparation, etc., but also the prepared ITO nanowires have good chemical stability, adjustable size, and can be produced Sequential arrangement overcomes the disadvantages of high cost, low yield, complex process and unfriendly environment in the preparation of nanowires in the prior art, and is suitable for many fields such as sensing, photovoltaics, electronics and information

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for digitally and controllably printing ITO (Indium Tin Oxide) nanowires
  • Method for digitally and controllably printing ITO (Indium Tin Oxide) nanowires
  • Method for digitally and controllably printing ITO (Indium Tin Oxide) nanowires

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0031] (1) mixing N,N-dimethylformamide and absolute ethanol with a mass ratio of 20:1, and configuring a mixed solvent;

[0032] (2) Dissolve polyvinylpyrrolidone, indium nitrate hydrate and stannous chloride dihydrate in a mixed solvent, stir at a temperature of 50 °C for 6 hours, and configure a precursor solution for printing; wherein, the mass ratio of polyvinylpyrrolidone is : indium nitrate hydrate=1:1.2, stannous chloride dihydrate: indium nitrate hydrate=1:6.5, in the precursor solution, the mass concentration of polyvinylpyrrolidone is 10.4%;

[0033] (3) Using an electro-fluidic printer to print the configured precursor solution as nanowires, wherein a high voltage of 0.65 kV is applied to the syringe needle, the distance from the syringe needle to the substrate is set to 2.5 mm, and the liquid flow rate of the syringe is set to 2.5 mm. Set to 50nL / min, and the moving speed of the substrate is set to 250mm / s;

[0034] (4) The printed nanowires are annealed at a hig...

Embodiment 2

[0037] (1) mixing N,N-dimethylformamide and absolute ethanol with a mass ratio of 10:1, and configuring a mixed solvent;

[0038] (2) Dissolve polyvinylpyrrolidone, indium nitrate hydrate and stannous chloride dihydrate in a mixed solvent, stir at a temperature of 50°C for 6 hours, and configure a precursor solution for printing; wherein, the mass ratio of polyvinylpyrrolidone is : indium nitrate hydrate=1:1.5, stannous chloride dihydrate: indium nitrate hydrate=1:10, in the precursor solution, the mass concentration of polyvinylpyrrolidone is 12%;

[0039] (3) Using an electrofluidic printer to print the configured precursor solution as nanowires, wherein a high voltage of 0.9 kV is applied to the syringe needle, the distance from the syringe needle to the substrate is set to 2 mm, and the liquid flow rate of the syringe is set to is 60nL / min, and the moving speed of the substrate is set to 200mm / s;

[0040] (4) The printed nanowires are annealed at a high temperature of 450...

Embodiment 3

[0042] (1) mixing N,N-dimethylformamide and absolute ethanol with a mass ratio of 5:1, and configuring a mixed solvent;

[0043] (2) Dissolve polyvinylpyrrolidone, indium nitrate hydrate and stannous chloride dihydrate in a mixed solvent, stir at a temperature of 25°C for 12 hours, and configure a precursor solution for printing; wherein the mass ratio of polyvinylpyrrolidone is : indium nitrate hydrate = 1:2, stannous chloride dihydrate: indium nitrate hydrate = 1:10, in the precursor solution, the mass concentration of polyvinylpyrrolidone is 9%;

[0044] (3) Using an electrofluidic printer to print the configured precursor solution as nanowires, wherein a high voltage of 1.1 kV is applied to the syringe needle, the distance from the syringe needle to the substrate is set to 3 mm, and the liquid flow rate of the syringe is set to is 30nL / min, and the moving speed of the substrate is set to 500mm / s;

[0045] (4) The printed nanowires are annealed at a high temperature of 550...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
diameteraaaaaaaaaa
lengthaaaaaaaaaa
electrical resistivityaaaaaaaaaa
Login to View More

Abstract

The invention relates to a method for digitally and controllably printing an ITO (Indium Tin Oxide) nano wire. According to the method, N, N-dimethylformamide and absolute ethyl alcohol are used as a mixed solvent, polyvinylpyrrolidone, indium nitrate hydrate and stannous chloride dihydrate are dissolved to prepare a precursor solution, then an ITO nano-wire array is printed through electrofluid printing equipment, and finally the ITO nano-wire is directly obtained through one-step high-temperature annealing. The prepared ITO nano wire has the advantages of being low in cost, high in yield, energy-saving, environment-friendly, simple in process, easy and convenient to operate, suitable for large-scale preparation and the like, and the prepared ITO nano wire is good in chemical stability, adjustable in size, capable of being arranged in order and suitable for multiple fields of sensing, photovoltaics, electronics, information and the like.

Description

technical field [0001] The invention relates to a method for digitally controllable printing of ITO nanowires, belonging to the field of advanced material manufacturing. Background technique [0002] As a wide bandgap (3.5-4.3 eV) semiconductor, indium tin oxide (ITO) has the advantages of good chemical stability and electrical conductivity, high transparency and acid and alkali corrosion resistance, and is widely used in sensing, photovoltaic, electronic and information fields. Usually, traditional ITO conductive electrodes are prepared by sputtering, electron beam evaporation and other processes. Not only are the equipment expensive and energy consumption high, but also the utilization rate of ITO targets is low, and there is a waste of rare metal element indium (In). In order to solve the above problems, people began to use the method of electrospinning to synthesize ITO one-dimensional nanowires with good electrical conductivity, which were applied to the preparation of...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityApplications(China)
IPC IPC(8): C03C17/23C04B41/87C04B35/453C04B35/622B28B1/00B33Y10/00B33Y70/10B33Y80/00B82Y30/00
CPCC03C17/23C04B41/505C04B41/87C04B41/009C04B35/453C04B35/62231B28B1/001B33Y10/00B33Y70/10B33Y80/00B82Y30/00C04B2235/3293C04B2235/6026C03C2218/11C04B41/5027C04B41/455C04B41/0072C04B35/10C04B35/14Y02P70/50
Inventor徐文涛屈尚达孙林
OwnerNANKAI UNIV