Environment friendly composite plastic ink and production process thereof
A composite plastic and ink technology, applied in ink, household utensils, applications, etc., can solve the problems affecting food hygiene and safety of packaging, affecting the health of operators, destroying the atmosphere, etc., achieving good mutual solubility, eliminating damage, and saving energy Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] Dissolve the modified chloroether resin solid with ethyl acetate, ethanol, isopropanol to make the modified chloroether resin liquid, wherein the weight percentage of ethyl acetate is 35%, the weight percentage of ethanol is 20%, and the weight percentage of isopropanol The percentage is 15%, and the weight percentage of the modified chloroether resin solid is 30%;
[0033] Use ethyl acetate, ethanol, isopropanol to dissolve the modified adhesion promotion resin solid to make the modified adhesion promotion resin liquid, wherein the weight percent of ethyl acetate is 40%, the weight percent of ethanol is 20%, isopropanol The weight percentage of the modified chloroether resin solid is 25% by weight.
[0034] A kind of environment-friendly composite plastic printing ink, its raw material component and weight percent are as follows:
[0035] Modified Chlorine Ether Resin Liquid 12%
[0036] Modified Adhesion Improvement Resin Liquid 4%
[0037] Pigment 28%
[0038] Fi...
Embodiment 2
[0051] Dissolve the modified chloroether resin solid with ethyl acetate, ethanol, isopropanol to make the modified chloroether resin liquid, wherein the weight percentage of ethyl acetate is 35%, the weight percentage of ethanol is 20%, and the weight percentage of isopropanol The percentage is 15%, and the weight percentage of the modified chloroether resin solid is 30%;
[0052]Use ethyl acetate, ethanol, isopropanol to dissolve the modified adhesion promotion resin solid to make the modified adhesion promotion resin liquid, wherein the weight percent of ethyl acetate is 40%, the weight percent of ethanol is 20%, isopropanol The weight percentage of the modified chloroether resin solid is 25% by weight.
[0053] A kind of environment-friendly composite plastic printing ink, its raw material component and weight percent are as follows:
[0054] Modified chloroether resin (solid) 15%
[0055] Modified adhesion promoting resin (solid) 5%
[0056] Pigment 10%
[0057] Filler...
Embodiment 3
[0070] Dissolve the modified chloroether resin solid with ethyl acetate, ethanol, isopropanol to make the modified chloroether resin liquid, wherein the weight percentage of ethyl acetate is 35%, the weight percentage of ethanol is 20%, and the weight percentage of isopropanol The percentage is 15%, and the weight percentage of the modified chloroether resin solid is 30%;
[0071] Use ethyl acetate, ethanol, isopropanol to dissolve the modified adhesion promotion resin solid to make the modified adhesion promotion resin liquid, wherein the weight percent of ethyl acetate is 40%, the weight percent of ethanol is 20%, isopropanol The weight percentage of the modified chloroether resin solid is 25% by weight.
[0072] A kind of environment-friendly composite plastic printing ink, its raw material component and weight percent are as follows:
[0073] Modified chloroether resin (solid) 8%
[0074] Modified adhesion promoting resin (solid) 1.5%
[0075] Pigment 30%
[0076] Fill...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com