A kind of high temperature acidifying corrosion inhibitor and preparation method thereof

A technology of acidizing corrosion inhibitor and corrosion inhibitor, applied in chemical instruments and methods, drilling composition and other directions, can solve the problems of operator's health damage, unsafe production process, increase of unit consumption of benzyl chloride, etc. Reduce production costs, reduce usage, and avoid the effect of self-condensation

Inactive Publication Date: 2012-02-15
SHOUGUANG YUXIN CHEM IND
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] During the reaction process, since the formaldehyde is in a sufficient state, it will inevitably cause the volatilization of formaldehyde. Usually, the consumption of formaldehyde is about 0.1255 tons for every ton of corrosion inhibitor produced, which is relatively large and the production cost is high. , the formaldehyde volatilized into the air has caused great damage to the health of the operators, and the production process is unsafe
[0005] In the production process, it is also necessary to add benzyl chloride and hydrochloric acid aqueous solution to the reaction kettle, resulting in relatively high moisture content in the reaction kettle, and benzyl chloride will undergo hydrolysis reaction, which increases the concentration of benzyl chloride in the quaternization reaction process. Unit consumption reduces the yield of the entire reaction. Usually, about 0.2066 tons of benzyl chloride is consumed for every ton of corrosion inhibitor produced, and the production cost is high.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of high temperature acidifying corrosion inhibitor and preparation method thereof
  • A kind of high temperature acidifying corrosion inhibitor and preparation method thereof
  • A kind of high temperature acidifying corrosion inhibitor and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0028] Example 1, take the following raw materials in parts by weight to produce a high-temperature acidification corrosion inhibitor, 79.33 parts of ethanol, 19 parts of formic acid, 22.33 parts of aniline, 31.11 parts of acetophenone, 26.13 parts of formaldehyde, 31.54 parts of benzyl chloride and 8.55 parts of propynyl alcohol share.

[0029] Produce according to the following process steps:

[0030] 1) The raw materials are prepared in parts by weight, and the formaldehyde is prepared into an aqueous solution with a concentration of 30%;

[0031] 2) Place ethanol, formic acid and aniline in the reaction kettle and stir for 8 minutes;

[0032] 3) Add acetophenone into the reaction kettle, raise the temperature of the reaction kettle to 80° C., then add formaldehyde solution to the reaction kettle dropwise, and the dropping time is 20 minutes;

[0033] 4) After adding the formaldehyde solution dropwise, control the temperature of the reactor at 80±0.5°C for 3 hours;

[00...

Embodiment 2

[0039] Embodiment 2, get the raw material production high temperature acidification corrosion inhibitor of following parts by weight, ethanol 83.5 parts, formic acid 20 parts, aniline 23.5 parts, acetophenone 32.75 parts, formaldehyde 27.5 parts, benzyl chloride 33.2 parts and propynyl alcohol 9 share.

[0040] Produce according to the following process steps:

[0041] 1) The raw materials are prepared in parts by weight, and the formaldehyde is prepared into an aqueous solution with a concentration of 30%;

[0042] 2) Place ethanol, formic acid and aniline in the reaction kettle and stir for 12 minutes;

[0043] 3) Add acetophenone into the reaction kettle, raise the temperature of the reaction kettle to 81° C., and then add formaldehyde dropwise to the reaction kettle for 30 minutes;

[0044] 4) After adding formaldehyde dropwise, control the temperature of the reactor at 78±0.5°C for 4 hours;

[0045] 5) Add benzyl chloride into the reactor, and control the temperature o...

Embodiment 3

[0050] Embodiment 3, take the raw material of following parts by weight to produce high-temperature acidification corrosion inhibitor: 87.68 parts of ethanol, 21 parts of formic acid, 24.68 parts of aniline, 34.39 parts of acetophenone, 28.88 parts of formaldehyde, 34.86 parts of benzyl chloride and 9.45 parts of propynyl alcohol share.

[0051] Produce according to the following process steps:

[0052] 1) The raw materials are prepared in parts by weight, and the formaldehyde is prepared into an aqueous solution with a concentration of 30%;

[0053] 2) Place ethanol, formic acid and aniline in the reaction kettle and stir for 18 minutes;

[0054] 3) Add acetophenone into the reaction kettle, raise the temperature of the reaction kettle to 82° C., then add formaldehyde solution dropwise to the reaction kettle, and the dropping time is 40 minutes;

[0055] 4) After adding the formaldehyde solution dropwise, control the temperature of the reactor at 77±0.5°C for 5 hours;

[0...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to a high-temperature acidification corrosion inhibitor and a preparation method thereof, comprising the following materials: 79.33-87.68 parts of ethanol, 19-21 parts of formic acid, 22.33-24.68 parts of aniline, 31.11-34.39 parts of acetophenone, and 26.13-28.88 parts of formaldehyde , 31.54-34.86 parts of benzyl chloride and 8.55-9.45 parts of propynyl alcohol, place ethanol, formic acid and aniline in the reaction kettle and stir, then add acetophenone into the reaction kettle, and then drop formaldehyde solution into the reaction kettle After adding the formaldehyde solution dropwise, add benzyl chloride into the reactor, lower the temperature of the reactor to room temperature, then add propynyl alcohol and stir. No need to add hydrochloric acid aqueous solution, the water content in the reactor is low, avoiding the hydrolysis of benzyl chloride, which is beneficial to reduce the unit consumption of benzyl chloride in the process of quaternization reaction, before adding formaldehyde dropwise, drop into the reactor The amount of formaldehyde is lower than the reaction molar ratio of synthetic Mannich base, and the formaldehyde is in a state of insufficient amount, which reduces the volatilization of formaldehyde, ensures the health of operators, and is safer.

Description

technical field [0001] The invention relates to a high-temperature acidification corrosion inhibitor and a preparation method thereof, which belong to the technical field of oil field chemical industry. Background technique [0002] In oil field construction, fracturing and acidizing is a very important oil production stimulation measure. Almost every oil production well has to go through this process. The commonly used acidizing agent is 20% hydrochloric acid or a compound of hydrochloric acid and hydrofluoric acid. Soil acid, these two acids are very strong inorganic acids, which will lead to corrosion of downhole pipe strings and metal equipment, and with the increase of well depth, the temperature will increase, which will inevitably lead to more serious corrosion. To prevent or reduce the corrosion of downhole tubing string by acid liquid at high temperature, it is necessary to add a high temperature corrosion inhibitor into the acid liquid. [0003] At present, common...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): C09K8/74
Inventor 杨明冯树海董景福杨磊
Owner SHOUGUANG YUXIN CHEM IND
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products