A technology of wool keratin and compound function, which is applied in the field of preparation of ITO/wool keratin solution compound function finishing agent, can solve problems such as waste and environmental impact, and achieve the effects of saving resources, protecting the environment and reducing costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] 1) Wash the wool with water, then wash it with detergent 209 for 30 minutes, then degrease it in ethanol-acetone mixed solvent (the volume ratio of ethanol and acetone is 1:1) for 5 hours, and finally crush it into a length of about 1 cm; Lotion formula, clean detergent 3 g / L, temperature 40°C, bath ratio 1:50. Add the washed raw material to 1-methyl-3-butylimidazolium chloride ionic liquid, wherein the raw material is 10% by weight of the ionic liquid, and dissolve under magnetic stirring for 4 hours at 100°C, Just can obtain the keratin / ionic liquid solution of corresponding concentration.
[0025] 2) Prepare indium trichloride weakly acidic solution with metal indium and hydrochloric acid at a molar ratio of 1:4, dry the water to obtain indium trichloride powder and dissolve it in acetylacetone with stirring at a concentration of 100g / L at 50°C Medium; Dissolve tin tetrachloride crystals in absolute ethanol at a concentration of 50 g / L at 30°C. Then, the indium tri...
Embodiment 2
[0028] 1) Wash the wool with water, then wash it with detergent 105 for 30 minutes, then degrease it in ethanol-acetone mixed solvent (the volume ratio of ethanol and acetone is 1.5:1) for 10 hours, and finally crush it into a length of about 2cm; Lotion formula, detergent 4 g / L, temperature 50°C, bath ratio 1:40. Add the washed raw material to 1-methyl-3-allylimidazolium chloride ionic liquid, wherein the raw material is 20% by weight of the ionic liquid, and dissolve under magnetic stirring at 110°C for 3.5 hours , the corresponding concentration of keratin / ionic liquid solution can be obtained.
[0029] 2) Prepare indium trichloride weakly acidic solution with metallic indium and hydrochloric acid in a molar ratio of 1:4, dry the water to obtain indium trichloride powder and dissolve it in acetylacetone at 60°C with stirring at a concentration of 110g / L Medium; Dissolve tin tetrachloride crystals in absolute ethanol at a concentration of 60 g / L at 20°C. Then the indium tr...
Embodiment 3
[0032] 1) Wash the wool with water, then wash it with detergent 6501 for 20 minutes, then degrease it in ethanol-acetone mixed solvent (the volume ratio of ethanol and acetone is 1.8:1) for 18 hours, and finally crush it into a length of about 3 cm; Lotion formula, detergent 5 g / L, temperature 60°C, bath ratio 1:30. Add the washed raw materials into 1-methyl-3-ethylimidazolium chloride ionic liquid, wherein the raw materials are 5% by weight of the ionic liquid, and dissolve under magnetic stirring at 120°C for 3 hours, and then Keratin / ionic liquid solutions with corresponding concentrations can be obtained.
[0033] 2) Prepare a weakly acidic solution of indium trichloride with metal indium and hydrochloric acid in a molar ratio of 1:3, dry the water to obtain indium trichloride powder, and stir and dissolve it in acetylacetone at a concentration of 120 g / L at 60°C. medium; tin tetrachloride crystals were dissolved in absolute ethanol at a concentration of 80 g / L at 25 °C. T...