Embodiment 1
[0041] The embodiment of the present invention provides a preparation method of using waste dander to prepare concrete water reducer, the method is realized through the following steps:
[0042] Step 1: Degradation of waste dander:
[0043] Take 1000 parts of clean waste dander in parts by mass, add 200 parts of water, heat up to 35°C, add 0.5 part of penetrant JFC, stir for 1 hour, then adjust the pH to 9.5 with 40% sodium hydroxide by mass fraction, add 1 Part 2709-alkaline protease was incubated and stirred for 6 hours to obtain a solution for degrading waste dander, which was lowered to room temperature for subsequent use;
[0044] Step 2: Preparation of water reducing agent:
[0045] Add 30 parts of formaldehyde with a mass fraction of 36% to the degraded dander solution prepared in step 1, raise the temperature to 40°C, add 2 parts of a 40% sodium hydroxide solution, and add in portions within 30 minutes 27~30 parts of urea, after adding, keep warm for 30 minutes, then...
Embodiment 2
[0047] The embodiment of the present invention provides a preparation method of using waste dander to prepare concrete water reducer, the method is realized through the following steps:
[0048] Step 1: Degradation of waste dander:
[0049] Take 120 parts by mass of clean waste dander, add 240 parts of water, heat up to 40°C, add 1 part of penetrant JFC, stir for 1.5 hours, then use 40% sodium hydroxide to adjust the pH to 10.5, add 1.2 parts 2709-alkaline protease, heat preservation and stirring for 8 hours to obtain a solution for degrading waste dander, and lower it to room temperature for later use;
[0050] Step 2: Preparation of water reducing agent:
[0051]Add 40 parts of formaldehyde with a mass fraction of 36% to the degraded dander solution prepared in step 1, raise the temperature to 50°C, add 5 parts of a 40% sodium hydroxide solution, and add in portions within 60 minutes Add 30 parts of urea, add 6 parts of sodium sulfite and keep warm for 60 minutes, then add...
Embodiment 3
[0053] The embodiment of the present invention provides a preparation method of using waste dander to prepare concrete water reducer, the method is realized through the following steps:
[0054] Step 1: Degradation of waste dander:
[0055] Take 110 parts by mass of clean waste dander, add 220 parts of water, heat up to 37.5°C, add 0.75 parts of penetrant JFC, stir for 1.25 hours, then use 40% sodium hydroxide to adjust the pH to 10, add 1.1 parts 2709-alkaline protease, insulated and stirred for 7 hours to obtain a solution for degrading waste dander, which was lowered to room temperature for later use;
[0056] Step 2: Preparation of water reducing agent:
[0057] Add 35 parts of formaldehyde with a mass fraction of 36% to the degraded dander solution prepared in step 1, raise the temperature to 45°C, add 3.5 parts of a 40% sodium hydroxide solution, and add in portions within 45 minutes 58 parts of melamine, add 45 parts of sodium bisulfite and keep warm for 45 minutes, t...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com