A kind of anti-counterfeiting paper made of raw paper and its preparation process
A technology of anti-counterfeiting paper and base paper, which is applied in special paper, paper, papermaking, etc., can solve the problems of poor anti-counterfeiting effect, high production cost and complicated process of anti-counterfeiting paper, and achieve the effect of not being easy to counterfeit, low production cost and simple process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] A process for making anti-counterfeiting paper using base paper, comprising the following steps:
[0029] 1) Use a 120-mesh anilox roller to coat a transparent laser PET film with a thickness of 12 μm and a highly transparent UV varnish, with a coating amount of 3g per square meter;
[0030] Wherein the highly transparent UV varnish comprises each component of the following parts by weight:
[0031] 10 parts of epoxy acrylic resin polymer, 10 parts of polyester acrylic resin polymer, 15 parts of trimethylolpropane triacetate, 5 parts of tripropylene glycol diacrylate, 2 parts of benzophenone, 0.1 part of photoinitiator , 10 parts of monofunctional methacrylate, 1 part of photoaccelerator. 2) Composite the transparent laser film obtained in 1) after being coated with highly transparent UV varnish with base paper with a weight of 28g per square meter and a water content of 3.0-3.6%, cured and dried under a 5KW UV lamp, Peel off the transparent laser film to obtain trans...
Embodiment 2
[0038] A process for making anti-counterfeiting paper using base paper, comprising the following steps:
[0039] 1) Use a 300-mesh anilox roller to coat a transparent laser BOPP film with a thickness of 24 μm with high-transparency UV varnish; the coating amount is 10g per square meter.
[0040] Wherein the highly transparent UV varnish comprises each component of the following parts by weight:
[0041] 20 parts of epoxy acrylic resin polymer, 20 parts of polyester acrylic resin polymer, 5 parts of trimethylolpropane triacetate, 3 parts of tripropylene glycol diacrylate, 5 parts of benzophenone, 1 part of photoinitiator , 5 parts of monofunctional methacrylate, 0.1 part of photoaccelerator.
[0042] 2) Composite the transparent laser film obtained in 1) after being coated with highly transparent UV varnish with the base paper with a weight of 400g per square meter and a water content of 4.5-5.0%, cured and dried under a 15KW UV lamp, Peel off the transparent laser film to ob...
Embodiment 3
[0049] A process for making anti-counterfeiting paper using base paper, comprising the following steps:
[0050] 1) Using a 210-mesh anilox roller, apply highly transparent UV varnish on a transparent laser BOPP film with a thickness of 18 μm; the coating amount is 6g per square meter.
[0051] Wherein the highly transparent UV varnish comprises each component of the following parts by weight:
[0052] 14 parts of epoxy acrylic resin polymer, 15 parts of polyester acrylic resin polymer, 10 parts of trimethylolpropane triacetate, 4 parts of tripropylene glycol diacrylate, 3.5 parts of benzophenone, 0.3 parts of photoinitiator , 7 parts of monofunctional methacrylate, 0.3 parts of photoaccelerator.
[0053] 2) Composite the transparent laser film obtained in 1) after being coated with highly transparent UV varnish with the base paper with a weight of 28-400g per square meter and a water content of 3.0-4.0%, and cure it under a 9KW UV lamp. Dry, peel off the transparent laser f...
PUM
| Property | Measurement | Unit |
|---|---|---|
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |