Embodiment 1
[0021] [Example 1] Preparation of polyacrylate / polysilane core-shell composite emulsion
[0022] 1. Synthesis of silanes containing styrenesulfonyltrimethoxysilyl sulfide comonomer
[0023] Silanes containing styrenesulfonyltrimethoxysilyl propyl sulfide comonomer were synthesized as follows:
[0024]
[0025] 2. Preparation of Core-Shell Polymerized Emulsion
[0026] 2.1 Monomer pre-emulsification
[0027] Mix a certain amount of deionized water and emulsifier, stir quickly to dissolve it, add butyl acrylate, methyl methacrylate, and silane containing styrenesulfonyl trimethoxysilyl propyl sulfide comonomer in turn, at 40 Stir at ℃ for 15 min to obtain a pre-emulsion.
[0028] 2.2 Semi-continuous dropwise addition
[0029] A four-neck flask equipped with an electric stirrer, a reflux condenser and a thermometer was placed in a constant temperature water bath, and the 15% pre-emulsion and APS initiator solution were stirred rapidly and gradually heated to 80° C. to obta...
Embodiment 2
[0030] [Example 2] Preparation of water-based traffic line marking paint
[0031] The formula of the water-based traffic line marking paint in this embodiment is: 8% rutile titanium dioxide, 30% core-shell polymer emulsion, 2% diethylenetriamine, 10% talcum powder, 10% barium sulfate, 15% kaolin, polyacrylic acid Sodium salt 1.5%, foam breaking polymer and polysiloxane solution 0.5%, triethylamine 2%, methanol 1%, bactericide 0.4%, nano silicon dioxide 1%, glass microspheres 5%, propylene glycol 2%, Deionized water was added to 100%.
[0032] Please refer to the attached figure 1 , the preparation method of the water-based traffic line marking paint of the present embodiment is:
[0033] (1) Add water, rutile titanium dioxide, dispersant, talcum powder, barium sulfate, kaolin, dispersant, and ammonium hydroxide into a container with a stirrer. After mixing, it is sent to a conical mill for grinding to make a color paste with a fineness of about 40 microns.
[0034] (2) Add...
Embodiment 3
[0036] [Example 3] Preparation of water-based traffic line marking paint
[0037] The formula of the water-based traffic line marking paint of this embodiment is: titanium yellow 12%, core-shell polymer emulsion 15%, diethylenetriamine 7%, talcum powder 15%, barium sulfate 10%, kaolin 5%, polyacrylic acid sodium salt 3.5%, foam breaking polymer and polysiloxane solution 1.1%, triethylamine 4%, methanol 3%, bactericide 0.9%, nano silicon dioxide 4%, glass beads 10%, propylene glycol 5%, deionized Water was added to 100%.
[0038] The preparation method of the present embodiment is identical with embodiment 2